Inconel 600 (UNS N06600): composition, properties and applications

Inconel 600 is the original 72 % nickel-chromium-iron workhorse: a solid-solution alloy with no ageing treatment, no chloride stress-corrosion cracking, and enough chromium to survive continuous service in air up to about 1,095 °C. It is the grade we quote most often for caustic evaporators, furnace internals and high-purity water systems — and the one most often confused with 601 and 690. This guide sets out the numbers, the service limits and the selection rules behind those quotes.

Machined nickel alloy forged discs

What Inconel 600 is — in one paragraph

Inconel 600 (UNS N06600, W.Nr 2.4816, NiCr15Fe) is a nickel-chromium-iron alloy with a minimum of 72 % nickel, 14–17 % chromium and 6–10 % iron. It has been in service since the 1930s and it is still the reference grade wherever three requirements meet at once: immunity to chloride stress-corrosion cracking, resistance to hot caustic alkalies, and oxidation resistance in air up to roughly 1,095 °C. It is a solid-solution alloy — there is no precipitation-hardening step, no ageing cycle and no condition to argue about on the purchase order beyond “annealed” or “cold-worked”.

The high nickel content is what does the corrosion work: nickel is thermodynamically stable in caustic and in neutral chloride solutions, so 600 does not crack the way 304 or 316 do when chlorides and residual stress combine. The chromium supplies the oxidation resistance and the passivity in oxidising acids. The iron is there for economy and for structural stability — it keeps the alloy fully austenitic with no sigma-phase risk in the normal service window.

Where 600 stops: it is not a pitting alloy. With no molybdenum, its pitting resistance equivalent (PREN ≈ 15–17) is no better than a 304, so seawater, chloride bleaches and wet chloride deposits will pit it. That single fact explains most of the grade confusion we see in enquiries — if the duty is chlorides in water, the answer is 625 or a super duplex, not 600.

Nominal chemical composition

Composition limits per ASTM B168 / B166 / B167 (UNS N06600), weight percent:

ElementContent (wt %)Why it matters
Nickel (Ni)72.0 minThe corrosion engine: immunity to chloride SCC, resistance to caustic and to high-purity water
Chromium (Cr)14.0–17.0Passive oxide film; oxidation resistance to ~1,095 °C; resistance to nitric and other oxidising acids
Iron (Fe)6.0–10.0Austenite stabiliser and cost balance; keeps the structure single-phase in service
Carbon (C)0.15 maxDeliberately higher than in 625 or 690 — some grain-boundary carbide gives creep strength, at the cost of mild sensitisation risk in the wrong medium
Manganese (Mn)1.0 maxDeoxidation during melting; sulfide shape control
Silicon (Si)0.5 maxDeoxidation; higher silicon would hurt weldability and hot ductility
Copper (Cu)0.5 maxResidual; capped because copper lowers hot workability
Sulphur (S)0.015 maxCapped for hot ductility and weld soundness

There is no molybdenum and no aluminium in 600. That is the whole difference in behaviour against 625 (Mo → pitting resistance) and against 601 (Al → oxidation resistance above 1,000 °C). When a customer asks for “the 600 that resists seawater”, the answer is that no such grade exists.

Mechanical properties

Room-temperature tensile properties, annealed condition. The middle column is the ASTM B168 / B166 acceptance minimum; the right-hand column is what we actually see on mill certificates for plate and bar.

Condition0.2 % yield strengthTensile strengthElongationHardness
Annealed — ASTM minimum≥ 240 MPa≥ 550 MPa≥ 30 %≤ 187 HB typical
Annealed — typical mill certificate240–345 MPa550–690 MPa30–45 %140–170 HB
Cold-worked / cold-drawn barBy agreement, typically 450–700 MPaBy agreement, typically 700–900 MPa≥ 12–20 % depending on reductionReported per heat

Notes for designers. Cold-worked 600 is not a standard supply condition — it only exists when you write the strength level into the order, and it comes with reduced elongation and a stress-relief question. For anything above 450 °C, hot-strength rather than room-temperature tensile governs the design: 600 holds useful strength to about 700 °C, but creep and rupture data must be used above roughly 550 °C, and above 700 °C the grade is usually the wrong tool next to 625, 617 or a cast heat-resistant alloy.

Impact and low temperature. 600 stays ductile down to cryogenic temperature — there is no ductile-to-brittle transition of the kind that limits ferritic steels, which is why it appears in LNG and cold-box piping where a nickel alloy is specified for other reasons.

Physical properties

PropertyValueComment
Density8.47 g/cm³About 8 % heavier than carbon steel — matters for weight-critical supports and lifting plans
Melting range1,354–1,413 °CSolidus–liquidus; welding and hot-working windows sit well below the solidus
Thermal conductivity≈ 14.9 W/m·K at 20 °C; ≈ 22 W/m·K at 500 °CRoughly one quarter of carbon steel at room temperature — expect steeper thermal gradients and slower heat-up
Specific heat≈ 444 J/kg·KUsed for heat-up and quench calculations
Thermal expansion (mean, 20–100 °C)≈ 13.3 ×10⁻⁶ /KRises to ≈ 15.3 ×10⁻⁶ /K over 20–600 °C; check dissimilar joints against the matching steel
Electrical resistivity≈ 1.03 µΩ·m at 20 °CRelevant for sheathed heater and thermocouple elements
Modulus of elasticity≈ 214 GPa at 20 °CFalls to roughly 160 GPa at 540 °C — allow for it in bellows and spring design
Magnetic behaviourEssentially non-magnetic (relative permeability ≈ 1.01; Curie point below −100 °C)Heavy cold work can raise the response slightly; that is normal and not a grade error

Corrosion and heat resistance — where 600 earns its keep

Caustic alkalies

This is 600's home ground. Sodium and potassium hydroxide, in concentrations and at temperatures where 304/316 would crack within months, are handled by 600 evaporator tubes, heating coils and caustic concentrator shells. The limitation to know: above roughly 300 °C in very high caustic concentrations, even 600 can suffer caustic stress-corrosion cracking in highly stressed cold-formed or welded areas — specify a stress-relieved condition (about 870–900 °C) for those duty points rather than assuming the annealed condition is enough.

Chloride stress-corrosion cracking

600 is effectively immune in the temperature and chloride range that destroys austenitic stainless steels. This is why it turns up in pulp-mill white liquor, in chloride-bearing process water and in food plants that clean with hypochlorite between campaigns. Immunity to SCC is not immunity to pitting: standing chlorides still need to be flushed.

High-purity and nuclear water

600 was the original PWR steam-generator tube material and still appears in reactor internals, pressuriser parts and primary-circuit instrumentation. Its service history is also the reason 690 exists: primary-water stress-corrosion cracking (PWSCC) appeared in 600 tubes at operating temperature, and the industry moved to the 30 % Cr grade. For new nuclear-primary work, expect 690 or 800 to be specified; 600 remains common in secondary circuits and in non-nuclear high-purity water.

Oxidation and high temperature

In dry air, 600 is used continuously to about 1,095 °C and intermittently a little higher, with good resistance to scaling and to carburisation. The critical caveat is atmosphere chemistry: in sulfur-bearing gases the usable temperature drops sharply (about 815 °C is the practical ceiling), and in strongly reducing atmospheres the protective Cr₂O₃ film cannot form at all.

Acids

Good in nitric acid across the usual concentrations, and in many organic acids. Not the right choice for hot concentrated sulphuric or hydrochloric acid, where the C-family alloys do the work.

Selection rule of thumb: caustic, high-purity water, chloride-SCC duty, or dry-air oxidation below 1,095 °C → 600. Add molybdenum (625) the moment the medium is seawater, chloride bleach or an oxidising chloride salt. Add aluminium (601) the moment the duty is oxidation or carburisation above 1,000 °C with thermal cycling.

Typical applications by industry

IndustryTypical 600 componentsWhy 600
Chemical / causticCaustic evaporator tubes and tube sheets, concentrator shells, heating coils, fatty-acid processing vesselsCaustic resistance plus chloride-SCC immunity
Heat treatment / furnacesMuffles, retorts, furnace belts, radiant-tube supports, quenching fixtures, thermocouple protection sheathsOxidation and carburisation resistance to ~1,095 °C, no phase instability on cycling
Nuclear / powerSteam-generator internals, pressuriser components, control-rod drive mechanisms, secondary-circuit tubingHigh-purity water compatibility, predictable elevated-temperature properties
Food & pharmaceuticalProcess vessels, heat-exchanger tubing, steriliser baskets, chloride-cleaning duty equipmentCleanliness, no copper or lead, tolerance of hypochlorite cleaning cycles
Aerospace & enginesExhaust liners, turbine seals, combustion-chamber supports, bellowsStrength and oxidation resistance in the 600–900 °C band
PetrochemicalCatalytic reformer internals, hydrotreater thermowells, flue-gas desulphurisation dampersMixed oxidising/sulphidising service at moderate temperature
Electrical / electronicsSheathed heating elements, cathode supports, spark-plug electrodesStable resistivity, non-magnetic, oxidation resistant

Standards and product forms we supply

Product formStandardTypical supply range
Plate, sheet, stripASTM B168 / ASME SB168; AMS 55400.5–100 mm plate; coil and cut-to-length sheet
Bar, rod, wireASTM B166 / ASME SB166; AMS 5665Dia 6–300 mm bar; wire to drawing
Seamless pipe and tubeASTM B167 / SB167Pipe to schedule; tube to drawing
Condenser / heat-exchanger tubeASTM B163 / SB1636–25 mm OD, wall by calculation
Welded tube and pipeASTM B516 / B517Thin-wall tube, large-diameter pipe
FittingsASTM B366Butt-weld and forged fittings
Forgings, flanges, blocksASTM B564To drawing, with 3.1 certification
Weld consumablesERNiCr-3 (AWS A5.14); ENiCrFe-3 (AWS A5.11)Wire, covered electrodes, strip for overlay

Designations to quote on the enquiry: UNS N06600 / W.Nr 2.4816 / NiCr15Fe / AFNOR NC 15 Fe / JIS NCF 600 / GB NS312 (cross-reference only — verify before ordering). European heat-resisting coverage sits under EN 10095; German flat-product and bar standards are DIN 17750 and DIN 17752–17754.

Fabrication, welding and purchasing notes

Forming and machining

  • 600 work-hardens quickly — roughly like 316L but with a steeper curve. Cold forming needs more power and more intermediate anneals; plan the bend radius from the annealed temper, not from a cold-rolled sheet.
  • Machining: carbide tooling, low surface speed, heavy feed, no dwell. The alloy galls, so sharp edges and a rigid set-up matter more than the insert grade.
  • Annealing for maximum corrosion resistance: 1,090–1,150 °C, then fast cool (water or rapid air) to keep carbides in solution. Stress relief, where needed for caustic service, is 870–900 °C.

Welding

  • No preheat. No post-weld heat treatment for general corrosion service — one of the practical reasons 600 is chosen over higher-strength nickel alloys.
  • Filler: ERNiCr-3 (FM 82) for TIG/MIG and submerged arc; ENiCrFe-3 (WE 182) for covered electrodes. The same filler joins 600 to 601, to 625 and to carbon steel.
  • Low heat input, stringer beads, interpass temperature below 150 °C, and a purge on the root for tube work. Pickle and passivate afterwards (HF/HNO₃ paste or bath) to restore the oxide film.
  • For caustic service above 300 °C, treat the weld as a stress raiser: grind flush, avoid unrelieved tack welds, and specify stress relief if the design allows it.

Purchasing checklist

  • State the condition (annealed or cold-worked) and the standard, not just the trade name — “Inconel 600” alone does not define mechanicals.
  • Demand EN 10204 3.1 certificates with the actual heat analysis, and ask for the grain size if the part is going into a furnace or a nuclear-adjacent application.
  • PMI (XRF) every piece before packing. 600, 601 and 690 are visually identical and cannot be separated by a magnet — all three are non-magnetic.
  • For plate destined for pressure equipment, confirm whether ASME SB168 with a U-stamp traceability package is required before rolling — adding it afterwards is expensive.

Buying Inconel 600 from Hangbo

We supply Inconel 600 plate, sheet, bar, seamless tube, welded tube, forgings and weld wire from Shanghai, with in-house saw cutting, waterjet blanking, turning and PMI verification. Every shipment leaves with an EN 10204 3.1 mill certificate matched to the heat number on the bundle, and we can add third-party inspection (SGS, BV, TUV) at the port of loading when the end user requires it.

Typical lead times: 7–15 days for stock plate and bar sizes, 25–40 days for forged or machined-to-drawing parts, 20–30 days for non-standard seamless tube. If you are comparing 600 against 601 or 625, send us the duty — medium, concentration, temperature, and whether the atmosphere is oxidising, carburising or sulphidising — and we will tell you which grade we would put our own name on.

Frequently asked questions

Is Inconel 600 magnetic?

No. Annealed 600 is essentially non-magnetic, with a relative permeability around 1.01 and a Curie point below −100 °C. Heavy cold work (deep drawing, cold-drawn bar) can produce a faint magnetic response; that is normal metallurgy, not a wrong grade. Inconel 600, 601 and 690 are all non-magnetic, so a magnet will never separate them — use PMI.

Inconel 600 or 601 — which one should I specify?

Decide from the failure mode you are designing against. If it is corrosion — caustic, high-purity water, chloride SCC, nitric acid — use 600: it has more nickel and better caustic resistance. If it is oxidation, carburisation or thermal cycling above 1,000 °C, use 601: its 1.0–1.7 % aluminium forms an Al₂O₃ scale that survives cycling far better than the Cr₂O₃ film on 600. Below 900 °C in clean oxidising service the two are close, and 600 is usually the cheaper buy.

Why did nuclear plants replace 600 with 690?

Primary-water stress-corrosion cracking (PWSCC) was found in Alloy 600 steam-generator tubing at operating temperature. Alloy 690 raises chromium from 14–17 % to 27–31 %, which pushes the crack-tip chemistry far enough to stop the mechanism, and the industry converted. 600 is still widely used in secondary circuits, non-nuclear high-purity water and dozens of non-nuclear duties — but for new nuclear primary work, expect 690 or 800 to be specified.

Can Inconel 600 be used in seawater?

No. With no molybdenum, 600 has a PREN of only about 15–17 and will pit and crevice-corrode in seawater, especially under deposits or in stagnant zones. Seawater duty needs 625 (PREN ≈ 50) or a super duplex such as 2507. 600's chloride resistance is resistance to stress-corrosion cracking, not to pitting — a distinction that catches a lot of buyers.

Does Inconel 600 need heat treatment after welding?

Not for general corrosion service: weld 600 with ERNiCr-3 filler, keep interpass below 150 °C, pickle and passivate, and it is ready. Stress relief at 870–900 °C is specified when the assembly sees hot caustic above roughly 300 °C, or when dimensional stability under thermal cycling matters. Note that stress relief is not a substitute for the correct grade — it reduces residual stress, it does not make 600 into a pitting alloy.

Need Inconel 600 (UNS N06600)?

Send us your drawing or specification for a quotation — we reply within one business day.

Request a quote