[email protected] WhatsApp +86 159 0085 2030 Qingpu, Shanghai Reply within 1 business day

Inconel 617 (UNS N06617): composition, properties and applications

Inconel 617 is the cobalt-bearing member of the Ni-Cr-Mo family, and the cobalt is the whole point: 10–15 % Co plus 8–10 % Mo in solid solution is what keeps 617 load-bearing at 800–950 °C, where 625 has already run out of creep strength. Add 1 % aluminium for a tenacious oxide scale and you get the standard combustor and intermediate-heat-exchanger alloy. This guide puts the numbers on the table — composition, tensile and 10,000-hour rupture data, the physical constants that matter for thermal-fatigue design, and the one comparison every buyer should run before paying for cobalt.

What Inconel 617 is — in one paragraph

Inconel 617 (UNS N06617, W.Nr 2.4663, NiCr23Co12Mo) is a solid-solution-strengthened nickel-chromium-cobalt-molybdenum alloy: roughly 22 % Cr, 12.5 % Co, 9 % Mo, 1.2 % Al, balance nickel (44.5 % min). There is no ageing treatment and no gamma-double-prime phase — the strength comes from Co and Mo dissolved in the austenitic matrix plus a controlled population of primary carbides from the deliberate 0.05–0.15 % carbon range. What makes 617 different from 625 is the temperature at which that strength survives: 625 is a corrosion alloy that happens to be heat resistant, while 617 was designed from the start as a load-bearing creep alloy for 800–950 °C, with an aluminium addition that holds an adherent Cr2O3 / Al2O3 scale under thermal cycling.

Three properties explain where you find it: it holds roughly 90 MPa of 10,000-hour rupture strength at 750 °C, it is one of very few wrought alloys qualified for impure-helium service in high-temperature gas-cooled reactors, and it stays metallurgically stable (no sigma-phase embrittlement) during tens of thousands of hours between 650 and 900 °C. It is also weldable without post-weld heat treatment, which is why combustor liners, transition ducts and reformer outlet manifolds are built from it rather than from a cast superalloy.

Chemical composition (ASTM B168 / B166)

ElementContent (wt %)Why it matters
Nickel (Ni)44.5 min (balance)Austenitic matrix; keeps toughness and weldability at temperature
Chromium (Cr)20.0–24.0Oxidation and hot-corrosion resistance; Cr2O3 scale former
Cobalt (Co)10.0–15.0Solid-solution strengthener — the single biggest reason 617 out-creeps 625 above 700 °C. Also the price driver
Molybdenum (Mo)8.0–10.0Solid-solution strength and resistance to reducing gases; raises creep activation energy
Aluminium (Al)0.8–1.5Forms a sub-scale of Al2O3 that pins the oxide and improves spalling resistance under cycling
Carbon (C)0.05–0.15Deliberately high: primary M23C6 / M6C carbides pin grain boundaries for creep. A low-carbon certificate is a red flag, not a bonus
Iron (Fe)3.0 maxResidual; higher Fe dilutes the solid-solution strengthening
Manganese (Mn)1.0 maxDeoxidation, sulphur control
Silicon (Si)1.0 maxMelt deoxidation; also affects weld pool fluidity
Titanium (Ti)0.6 maxMinor carbide former; not an age-hardening addition at this level
Copper (Cu)0.5 maxResidual
Boron (B)0.006 maxGrain-boundary cohesion, creep ductility
Sulphur (S)0.015 maxTramp element — low S matters for weldability and hot ductility

The European designation 2.4663 / NiCr23Co12Mo is close but not identical: EN narrows Cr to 20.0–23.0, Co to 11.0–14.0 and C to 0.05–0.10, and tightens Mn and Si to 0.2 % max. A dual-certified heat therefore has to sit inside the intersection. If your design is based on ASME allowable stresses, order to the ASME/ASTM specification, not to the EN grade.

Mechanical properties — room temperature and hot

Delivery condition for every product form is solution annealed (typically 1,170–1,180 °C, rapid cool). Minimum values per ASTM B168 (plate, sheet, strip) are modest because the alloy is designed for creep, not for room-temperature yield — the typical mill values run far above them:

Condition / form0.2 % yield (MPa)Tensile (MPa)ElongationHardness
ASTM B168 plate / sheet — minimum≥ 240≥ 655≥ 30 %—
ASTM B166 bar — minimum≥ 240≥ 655≥ 30 % (35 % quoted by some mills)—
Hot-rolled plate, solution treated — typical32273462 %≈ 172 HB
Hot-rolled bar, solution treated — typical31876956 %≈ 181 HB
Cold-rolled sheet, solution treated — typical35175558 %≈ 173 HB
Cold-drawn tube, solution treated — typical38375856 %≈ 193 HB

The design-relevant curve is the hot one. Typical short-time tensile values for solution-annealed 617:

Temperature0.2 % yield (MPa)Tensile (MPa)Elongation
20 °C≈ 367≈ 77952 %
540 °C≈ 254≈ 61867 %
650 °C≈ 239≈ 62767 %
760 °C≈ 245≈ 48392 %
870 °C≈ 207≈ 28699 %
980 °C≈ 111≈ 15593 %
1,095 °C≈ 58≈ 7991 %

Note the yield plateau between 540 and 760 °C: it is not a typo. Carbide precipitation and short-range ordering offset thermal softening in that window, which is exactly the window 617 is bought for. Above 900 °C the drop becomes steep, and above 1,000 °C the alloy is a refractory-grade material, not a structural one.

Creep-rupture is where the money is. Stress to cause rupture, MPa:

Temperature10,000 h100,000 h
600 °C260190
650 °C170125
700 °C12395
750 °C9065
800 °C6545
850 °C4527
900 °C3016
1,000 °C10≈ 4.5 (estimated)

Data from the VDM Metals 617 datasheet (2021); the 1,000 °C / 100,000 h figure is an extrapolation and is marked as such. These are rupture stresses, not allowable design stresses — for those use the current ASME Code Case or VdTÜV 485 tables.

Physical properties

PropertyValueNotes
Density8.36 g/cm³Consistent across Special Metals, VDM and Haynes data
Melting range1,330–1,380 °CSolidus 1,330 °C, liquidus 1,380 °C; some sheets quote 1,332 °C solidus
Thermal conductivity13.4 W/m·K at 20 °C; 17.7 at 300 °C; 22.5 at 600 °C; 28.7 at 1,000 °CCalculated values in the source data — use for analysis, not acceptance
Specific heat419 J/kg·K at 20 °C; 561 at 600 °C; 662 at 1,000 °CCalculated values
Mean expansion coefficient11.6 ×10⁻⁶ /K (20–100 °C); 13.1 (20–300); 14.0 (20–600); 16.3 (20–1,000)Mean from ~26 °C to temperature, not instantaneous
Young's modulus211 GPa at 25 °C; 173 at 600 °C; 157 at 800 °C; 139 at 1,000 °CDynamic method; falls ~34 % by 800 °C — do not use 211 GPa in hot deflection calcs
Poisson's ratio0.30 (0.31–0.32 above 1,000 °C)
Electrical resistivity1.222 µΩ·m at 20 °C≈ 122 µΩ·cm; useful for eddy-current sorting
Magnetic behaviourEssentially non-magneticPermeability < 1.005; a magnet will stick slightly after heavy cold work

Two consequences for design. First, the expansion coefficient of 617 (11.6 ×10⁻⁶ /K to 100 °C, 16.3 to 1,000 °C) is lower than 600/601/800H and close to Hastelloy X, so dissimilar joints to austenitic stainless create a real thermal-stress gradient at 800 °C. Second, thermal conductivity of 13–14 W/m·K at working temperature means slow through-thickness heat transfer: thick 617 sections need controlled heating and cooling rates, and welding heat input must be managed to avoid steep gradients in the HAZ.

High-temperature resistance and where it stops

  • Oxidation: excellent. The Cr2O3 scale is backed by aluminium, giving good spalling resistance under thermal cycling to about 980 °C, and useful short-term exposure up to roughly 1,100 °C where mechanical load is low. Long-term load-bearing service belongs below 1,000 °C.
  • Carburisation: good in carbon-containing process gases, better than plain Ni-Cr grades because the Al-rich sub-scale slows carbon ingress — but not immune, and not a substitute for a proper protective atmosphere in a carburising furnace.
  • Nitriding: the weak point. Under high nitriding potential, aluminium nitride can form beneath the surface, and the resulting hardened, crack-prone layer is a fatigue initiator. VDM's own datasheet flags this caveat. For nitriding furnaces and ammonia-burner hardware, Haynes 230 is the correct choice, not 617.
  • Sulphidation: moderate. Cobalt-base alloys (Haynes 188, L-605) and 230 are better in high-sulphur fuel ash and reducing sulphur atmospheres; 617 is not the answer for heavy-fuel-oil combustion with high Na/V/S.
  • Chlorination and HCl: not its job. 617 is a heat-resistant alloy with incidental aqueous corrosion resistance; for wet chlorine, hypochlorite or hot HCl use C-276 / C-22 or a reactive metal.
  • Aqueous corrosion: good in nitric acid and in oxidising salt solutions, which is why nitric-acid catalyst grids are a classic 617 application; adequate in many organic acids; not competitive with the C-family in reducing acids.

Selection rule. Up to ~650 °C with a wet, corrosive medium: buy 625 — it is cheaper and its pitting resistance is far higher. From ~700 to ~950 °C with sustained load: buy 617, because 625's creep strength collapses in that window (its 100,000 h rupture stress at 870 °C is about two-thirds of 617's). Above ~1,000 °C, in nitriding atmospheres, or where the part sees thousands of thermal cycles: step up to Haynes 230. And if the gas is sulphur-rich, go cobalt-base instead of either.

Comparing the two alloys on the same basis (stress for 10,000 h rupture, MPa):

TemperatureInconel 617Haynes 230Practical reading
650 °C170200230 leads by ~18 %
760 °C≈ 85 (interpolated)98230 leads by ~15 %
870 °C≈ 39 (interpolated)43Broadly equivalent
980 °C≈ 13 (interpolated)11Broadly equivalent; both marginal for load

617 values interpolated from the VDM 10,000 h table; 230 values from the Haynes 100 / 1,000 / 10,000 h table. The two alloys are close in creep — so the decision usually turns on atmosphere (230 for nitriding), on code coverage, on thickness availability and on price, not on strength alone.

Typical applications by industry

IndustryTypical 617 componentsWhy 617
Power generation — gas turbinesCombustor cans and liners, transition ducts, flame holders, sealing ringsCyclic oxidation resistance plus creep strength at 850–950 °C
Nuclear — HTGR / Gen IVIntermediate heat exchanger tubing, hot-gas ducts, control-rod componentsMetallurgical stability in impure helium at ~950 °C; the reference alloy for very-high-temperature reactor designs
Ultra-supercritical and A-USC boilersSuperheater / reheater tubing, headers, steam piping for 700 °C steamCreep strength at 700–760 °C where 617 and 740-class alloys compete
Petrochemical / syngasReformer outlet manifolds and pigtails, catalyst tubes, hot transfer linesCarburisation and oxidation resistance under pressure at 900–1,000 °C
Nitric acidCatalyst grids and support structuresOxidising-acid corrosion plus hot strength to carry the platinum gauze
Aerospace / rocketCombustion chambers, thrust-chamber liners, afterburner components, bellowsHigh-temperature fatigue and oxidation with weldability in thin sections
Industrial heat treatingRetorts, muffles, radiant tubes, fixtures, thermocouple protection tubesLong-life oxidation resistance at 950–1,100 °C with low load

Standards and product forms

  • Plate, sheet, strip: ASTM B168 / ASME SB168 (DIN 17750)
  • Rod, bar, wire: ASTM B166 / ASME SB166 (DIN 17752); AMS 5887 for aerospace bar and wire
  • Seamless pipe and tube: ASTM B167 / ASME SB167 (DIN 17751)
  • Welded tube: ASTM B516 / ASME SB516; welded pipe: ASTM B546
  • Forgings: ASTM B564 / ASME SB564 (DIN 17754) — flanges, rings, blocks, discs
  • Fittings: ASTM B366
  • Weld consumables: ERNiCrCoMo-1 (AWS A5.14) wire; ENiCrCoMo-1 (AWS A5.11) covered electrodes
  • Design codes: ASME Code Case 1956 (Section I and VIII Div. 1 allowable stresses); VdTÜV 485 for European pressure equipment; ASME Section III Div. 5 for very-high-temperature reactor components
  • European / other designations: W.Nr 2.4663, NiCr23Co12Mo, BS NA50, ISO NW6617

We supply 617 as plate from 0.5 mm to 60 mm, round bar and peeled bar, seamless tube and pipe, forged rings and blocks to drawing, and matching ERNiCrCoMo-1 filler. Every heat ships with EN 10204 3.1 certification and PMI verification.

Fabrication, welding and buying notes

Heat treatment. Solution anneal at 1,170–1,180 °C and cool rapidly — water or fast air depending on section. This is both the supply condition and the restoration treatment after hot forming or heavy cold work. There is no ageing step; anyone offering an aged 617 is describing a different alloy or a research variant.

Hot forming. Work in the 1,010–1,205 °C range, finish above roughly 950 °C, and charge into an already-hot furnace. Sulphur, lead, zinc and copper contamination on the surface will cause grain-boundary penetration at these temperatures — clean the part and use sulphur-free marking crayons.

Cold forming. 617 work-hardens quickly. Plan inter-stage anneals at about 1,040 °C, and remember that cold work raises room-temperature strength while consuming creep ductility — a cold-formed 617 part is not the same material as the annealed plate it came from.

Welding. GTAW, GMAW, plasma and SAW all work, with ERNiCrCoMo-1 matching filler (ENiCrCoMo-1 electrode). No preheat, no post-weld heat treatment for service up to about 900 °C. Weld in the solution-annealed condition, keep interpass temperature below 150 °C and use low heat input on the root: 617 is less prone to strain-age cracking than 718 or Waspaloy, but heavy restrained sections still crack if you weld on cold-worked or partially aged material. Purge the root and back-purge pipe; pickling after welding needs a nitric-hydrofluoric bath and should follow mechanical removal of the heat tint.

Machining. Austenitic and work-hardening: carbide tooling, positive rake, low surface speed, heavy feed that stays under the hardened skin, and generous coolant. Expect roughly 718-class tool life, not 316-class.

Buying checklist.

  • Write UNS N06617 plus the product standard (B168 vs B166 vs B167 vs B564) — the minimum mechanical values and tolerances differ by form.
  • Confirm carbon is inside 0.05–0.15 %. A 0.02 % carbon heat is not 617, and it will under-perform in creep.
  • For creep-critical parts, ask for grain size (typically ASTM 3–6) and state it on the PO; fine grain raises room-temperature strength and lowers creep life.
  • Use XRF/PMI to check cobalt at ~12 %. Co is the cleanest way to separate 617 from 625 (0 % Co), 601 (0 % Co) and Hastelloy X (0.5–2.5 % Co).
  • Expect cobalt-price exposure: 10–15 % Co means the alloy tracks the cobalt market, and quotes are usually valid for a shorter window than for 625. Lock the price or accept a metal-pass-through clause.
  • Lead time is the real constraint on 617, not price — wide plate and heavy bar are thin on the ground worldwide. Confirm the mill's rolling schedule before promising a delivery date.

Frequently asked questions

Is Inconel 617 age hardenable?

No. 617 is a solid-solution alloy; it is supplied solution annealed and never aged. Its strength comes from cobalt and molybdenum in solution plus primary carbides. If a specification demands an ageing treatment, it is not a 617 specification.

Inconel 617 versus Inconel 625 — how do I choose?

By temperature and medium. Below about 650 °C in a corrosive liquid or seawater, 625 wins on price and pitting resistance. Above 700 °C with sustained load, 625's creep strength falls away and 617 is the correct alloy. For hot concentrated reducing acids neither is right — that is C-276 / C-22 territory.

What filler metal do I weld 617 with?

ERNiCrCoMo-1 wire (AWS A5.14) or ENiCrCoMo-1 covered electrodes, matching composition. No preheat and no post-weld heat treatment are needed for service up to about 900 °C; weld in the solution-annealed condition.

What is the maximum service temperature of 617?

Roughly 980 °C for continuous, load-bearing, cyclic service; short-term exposure to about 1,100 °C is possible where stress is low and the atmosphere is clean and oxidising. Above 1,000 °C the alloy is no longer a structural material, and it should not be used in high-nitriding atmospheres at any temperature.

Is 617 magnetic?

No. It is austenitic and essentially non-magnetic, with permeability below 1.005. A slight magnet response after severe cold work is normal and does not indicate the wrong grade.

617 or Haynes 230 for a furnace retort at 1,050 °C?

Haynes 230, unless the atmosphere is sulphur-rich (then a cobalt-base alloy). 230 has comparable creep strength, distinctly better nitriding resistance and oxidation resistance to 1,150 °C, and no cobalt exposure in its price.

Need Inconel 617 (UNS N06617)?

Send us your drawing or specification for a quotation — we reply within one business day.

Request a quote