[email protected] WhatsApp +86 159 0085 2030 Qingpu, Shanghai Reply within 1 business day

904L (UNS N08904): the super-austenitic stainless built for sulphuric acid

904L (UNS N08904, EN 1.4539, W.Nr 1.4539) is the copper-bearing super-austenitic stainless steel: 25 % nickel, 21 % chromium, 4.5 % molybdenum and — the detail that defines the grade — 1.5 % copper. That copper is what makes 904L the standard material for sulphuric and phosphoric acid across the full concentration range at moderate temperature, and it is why 904L keeps winning work that 316L and 317L lose to general corrosion rather than to pitting. This guide sets out the composition logic, the mechanical and physical data, the corrosion envelope including its limits, and the fabrication rules that decide whether a 904L job passes hydrotest and survives the first decade.

Super austenitic piping at a desalination plant

What 904L is — in one paragraph

904L is a high-nickel, copper-alloyed austenitic stainless steel — the original "super-austenitic", developed in the 1960s for sulphuric acid service and still the reference grade for that duty. The 23–28 % nickel keeps the structure fully austenitic and gives excellent chloride stress-corrosion resistance; the 19–23 % chromium provides the passive film; the 4–5 % molybdenum raises pitting resistance to a PREN of about 35; and the 1–2 % copper is what allows it to resist sulphuric acid over the entire 0–100 % concentration range at temperatures up to roughly 35–40 °C, a claim neither 316L nor 254SMO can make.

Compared with 316L it is roughly twice the nickel, twice the molybdenum, three times the cost, and in the right medium a completely different service life. Compared with 254SMO it has less pitting resistance (PREN 35 vs 43) but more nickel and the copper advantage in reducing acids — so the two grades are complementary, not competing. The usual mistake we see in enquiries is a buyer specifying 904L for warm seawater, where 254SMO or a duplex grade would perform better for the same money.

Practical envelope: superb in sulphuric, phosphoric and organic acids, good in chlorides at moderate temperature, non-magnetic in all conditions, tough to −196 °C, and limited to about 400 °C by sigma-phase precipitation.

Chemical composition and what each element does

ASTM / EN limits in wt %. Note that EN 1.4539 is narrower than UNS N08904 on the two elements that matter most — see the purchasing section before ordering a dual-certified item.

ElementContent (wt %)Why it is there
Nickel (Ni)23.0–28.0Stabilises the fully austenitic structure, gives chloride SCC resistance, keeps toughness at cryogenic temperature
Chromium (Cr)19.0–23.0Passive film; general corrosion and oxidising-acid resistance
Molybdenum (Mo)4.0–5.0Pitting and crevice resistance in chlorides; strength in reducing acids
Copper (Cu)1.0–2.0The defining addition — catalytic/electrochemical effect that gives sulphuric acid resistance across all concentrations
Carbon (C)0.020 maxUltra-low carbon: no sensitisation in the weld HAZ, no PWHT needed
Manganese (Mn)2.00 maxDeoxidation and nitrogen solubility
Silicon (Si)1.00 maxDeoxidation; kept below the level that promotes sigma
Phosphorus (P)0.045 max (0.030 typical)Residual — embrittles if high
Sulphur (S)0.035 max (0.010 in EN)Residual — low sulphur improves weld soundness and hot ductility
Nitrogen (N)0.10 max (residual)Not a strengthening element here, unlike 254SMO: 904L gets its strength from nickel and molybdenum instead
Iron (Fe)balanceMatrix

PREN (Cr + 3.3 Mo + 16 N) with 21 % Cr and 4.5 % Mo and negligible nitrogen gives ≈ 35.9 — published data sheets quote 34–36. That places 904L clearly above 317L (≈ 32) and 316L (≈ 25), and clearly below the 6 % Mo super-austenitics (≈ 43). Remember that PREN only describes pitting resistance; it says nothing about acid resistance, which is where 904L's copper earns its keep.

Mechanical properties by product form

904L is supplied solution-annealed and is not hardenable by heat treatment. Because it is fully austenitic with no ferrite, seamless and welded product reach essentially the same values after annealing — the weld is not the weak link.

Product form / condition0.2 % yieldTensile strengthElongationHardness
Plate & sheet, annealed (ASTM A240 / B625)≥ 220 MPa≥ 490 MPa≥ 35 %≤ 220 HB
Seamless pipe & tube, annealed (ASTM A312 / B677)≥ 220 MPa≥ 490 MPa≥ 35 %70–90 HRB typical
Bar, annealed (ASTM B649 / A479)≥ 220 MPa≥ 490 MPa≥ 35 %≤ 220 HB
Typical mill values, annealed plate250–320 MPa550–660 MPa45–55 %130–180 HB
Cold-worked (20 % reduction) — typical500–600 MPa750–850 MPa20–30 %—

Design notes:

  • Low yield for a "super" alloy. At 220 MPa minimum, 904L is not a structural material — it is selected for corrosion duty, and wall thickness is set by corrosion allowance and by handling stiffness, not by pressure. Where you need both strength and this chemistry, 254SMO (300+ MPa) or a duplex grade is the better answer.
  • Ductility is exceptional: elongation of 45–55 % in the annealed condition makes 904L a favourite for deep-drawn parts, bellows, expansion joints and tube bending with tight radii.
  • Toughness to −196 °C. No ductile-brittle transition; 904L is used in cryogenic piping and LNG-adjacent equipment precisely for this.
  • Temperature ceiling ≈ 400 °C. Above 400 °C, and especially in the 400–600 °C band, sigma phase precipitates rapidly and both toughness and corrosion resistance fall. ASME BPVC Section VIII lists allowable stresses for 904L only up to about 371 °C, which is consistent with that limit. Sustained high-temperature service is not this grade's job.

Physical properties

PropertyValueComment
Density8.00 g/cm³ (7.95 in some mill data)Use 8.0 for mass and pressure calculations
Melting range≈ 1,350–1,400 °CSolidus–liquidus values of 1,300–1,390 °C are also published; the difference is immaterial to welding practice
Thermal conductivity, 20 °C≈ 12 W/m·KHalf that of carbon steel — heat concentrates at the weld, distortion is the main fabrication risk
Specific heat capacity≈ 450–500 J/kg·K20–100 °C; sources differ slightly, use 500 for conservative heat-input calculations
Mean thermal expansion, 20–100 °C≈ 15.0 ×10⁻⁶ /KBelow 254SMO (16.5) and close to 316L; still ~1.5× carbon steel
Modulus of elasticity, 20 °C≈ 195 GPa (190–210 published)Lower stiffness than carbon steel — check deflection on long spans
Electrical resistivity, 20 °C≈ 0.85–0.95 µΩ·mPublished values vary by source; not design-critical
Magnetic behaviourNon-magnetic in the annealed conditionBecause the structure is fully austenitic and highly alloyed, 904L stays essentially non-magnetic even after cold work and welding — an advantage over 316L in instrument and pharmaceutical applications

The high nickel content and low conductivity together mean that 904L responds sluggishly to induction heating and resists electrical resistance welding — relevant if you are welding tube-to-tubesheet by resistance methods or using induction bending.

Corrosion resistance — including where 904L stops

Sulphuric acid — the reason 904L exists

904L resists sulphuric acid over the full 0–100 % concentration range at temperatures up to roughly 35–40 °C, and in dilute acid (up to about 10–20 %) at appreciably higher temperatures. This is the copper effect: copper lowers the overpotential for the cathodic reduction reaction and promotes passivation in what is otherwise a strongly reducing acid. 316L, 317L and even 254SMO cannot match this — in dilute sulphuric acid at 60 °C, 316L corrodes at millimetres per year while 904L remains passive.

Phosphoric acid and mixed acids

Good resistance to wet-process and purified phosphoric acid, including the chloride- and fluoride-contaminated grades encountered in fertiliser plants, and to mixtures of sulphuric and nitric or acetic acid. Nitric acid service is better served by 310L-type or 904L depending on concentration — check the specific isocorrosion diagram.

Chlorides — good, but not a seawater alloy

With PREN ≈ 35, 904L has moderate pitting and crevice resistance: roughly a critical pitting temperature of 50–60 °C in ASTM G48 testing, and a critical crevice temperature around 30–40 °C. That is a large step above 316L and perfectly adequate for chloride-contaminated acids and for ambient seawater, but it is not a material for warm chlorinated seawater. For sea water above about 40 °C, specify 254SMO (PREN 43) or a super duplex grade.

Chloride stress-corrosion cracking resistance, however, is excellent: the 25 % nickel and fully austenitic structure push the SCC threshold well above 316L, which is why 904L is used for chloride-bearing process streams at 60–100 °C where 316L would crack.

Other media

  • Organic acids (acetic, formic, citric): very good, a standard material for acetic acid plants.
  • Sea water and brines: acceptable at ambient temperature and low velocity; not for hot aerated brine.
  • Hydrochloric acid: not suitable at any meaningful concentration — use Hastelloy B-2/B-3 or C-276.
  • Caustic: good to moderate concentrations; AL-6XN or nickel 200 are better at high concentration and temperature.
  • Intergranular corrosion: the 0.02 % maximum carbon effectively eliminates sensitisation, so welded 904L passes Strauss and Huey-type tests without PWHT.

Selection rule: 904L is an acid alloy, not a seawater alloy. Choose it when the medium is sulphuric or phosphoric acid at moderate temperature, or an acid with chlorides where 316L fails by general corrosion. When the problem is pitting in warm chloride water, go to 254SMO or 2507; when the acid is hot and reducing (HCl, concentrated H₂SO₄ above 60 °C), go to C-276 or Alloy 20 depending on oxidiser content.

Applications by industry

IndustryTypical 904L componentsWhy the grade is specified
Chemical processingSulphuric acid storage tanks, coolers, heat-exchanger tubing, reactor vessels, pump and valve bodies, pickling-line equipmentGeneral corrosion resistance across the full H₂SO₄ concentration range at moderate temperature; the copper addition is decisive
Fertiliser / phosphoric acidWet-process phosphoric acid evaporators, slurry piping, filter trays, agitator shaftsChloride- and fluoride-contaminated phosphoric acid at 80–120 °C
Pharmaceutical & fine chemicalsReactors, centrifuge baskets, fermentation vessels, CIP circuits, purified-water pipingNon-magnetic, ultra-low carbon, easily cleaned and passivated; good in mixed organic/inorganic acids
Oil & gas / petrochemicalHeat-exchanger tube bundles in refinery overheads, sour-water stripper internals, flue-gas ductingChloride SCC resistance at 60–100 °C where 316L cracks
Pulp & paperDigester and diffusion-washer components, chlorine-dioxide stage pipingChloride and chlorine-bearing liquors at moderate temperature
Environmental / FGDAbsorber linings, ductwork, stack gas reheat tubing, wastewater neutralisationAcid condensates with chlorides; weldable without PWHT
Marine & cryogenicExpansion bellows, flexible hoses, instrument tubing, LNG-adjacent pipingNon-magnetic, tough to −196 °C, good fatigue life in cyclic service

One pattern worth noting from our own order book: 904L is frequently specified for bellows and expansion joints. The combination of 45–55 % elongation, non-magnetic behaviour and acid resistance makes it the default answer for thin-wall formed components in chemical plants — and it is one of the few grades where the forming properties, not the corrosion data, decide the sale.

Standards and product forms

Product formSpecificationRemarks
Plate, sheet, stripASTM A240 / ASME SA-240; ASTM B625; EN 10088-2 (1.4539)B625 is the nickel-alloy route and is often quoted alongside A240
Seamless pipe & tubeASTM A312 / ASME SA-312; ASTM A213; ASTM B677Schedules 5S to 80S typical
Welded pipe & tubeASTM A249, A269, A358, B674Weld must be over-alloyed (ER385)
Bar, rod, billetASTM B649; ASTM A276 / A479B649 is the nickel-alloy bar specification for N08904
Forgings and fittingsASTM B564 (to drawing); ASTM A403 where applicableConfirm the forging grade on the certificate
Weld consumablesAWS A5.14 ER385; AWS A5.11 E385-15 / -16 / -17Never 308L or 316L — insufficient alloy, hot-cracking risk
European equivalentsEN 1.4539 (X1NiCrMoCu25-20-5); AFNOR Z2 NCDU 25-20; JIS SUS890LNote the narrower Cr/Ni windows versus ASTM — see purchasing
Code listingASME BPVC Section VIII Div. 1 (allowable stress to ≈ 371 °C)Verify allowable values in the current code edition

904L was originally a Uddeholm grade, now part of Outokumpu; the name is a trade designation, so the purchasing reference is UNS N08904. In Europe the same material is 1.4539, in Japan SUS890L, in France Z2 NCDU 25-20. All of these are the same chemistry family — but only the UNS number plus the certified heat analysis tells you what you actually received.

Fabrication, welding and heat treatment

Welding

  • Filler metal: ER385 / E385 only. 308L and 316L fillers are a recurring and expensive mistake — the weld metal is under-alloyed, loses corrosion resistance and cracks.
  • Hot-cracking risk is real. 904L solidifies as a fully austenitic structure with essentially zero ferrite, which makes it more sensitive to solidification cracking than 316L or duplex. Control heat input, avoid high-restraint joint designs, use a slight weave rather than a deep narrow bead, and keep interpass temperature below 150 °C.
  • No preheat, no PWHT. The 0.02 % carbon removes the sensitisation problem, so post-weld annealing is only needed after cold work or if the material has been held in the sigma range.
  • Back purge with argon on the root and clean, dedicated stainless tooling. Iron contamination is the usual cause of "unexplained" pitting on 904L welds.
  • Post-weld cleaning: pickle and passivate. On a heat-tinted surface the passive film is depleted in chromium and molybdenum and will pit in service.

Forming and machining

  • Cold forming is easier than 254SMO and closer to 316L, with high ductility — this is one of 904L's practical advantages for bellows, dished heads and tube bending.
  • Machining is "gummy" and work-hardens quickly: sharp positive-rake tools, constant feed, never rub, generous cutting fluid. Expect roughly 40–50 % of the machinability of 316L.
  • After more than about 15 % cold reduction, solution anneal if corrosion resistance is critical; otherwise the strain-induced martensite and residual stress will reduce performance.

Heat treatment

Solution anneal at 1,090–1,175 °C followed by rapid cooling (water quench for section thicknesses where it can be achieved, otherwise forced air). Avoid the 400–600 °C band entirely: sigma phase forms quickly there and does not dissolve below about 1,000 °C. Stress-relief annealing is not recommended as a substitute because it does not restore a damaged microstructure.

Purchasing notes — the dual-certification trap

  • The EN window is narrower than the ASTM window. EN 1.4539 requires Cr 19.0–21.0 % and Ni 24.0–26.0 %, while UNS N08904 allows Cr 19.0–23.0 % and Ni 23.0–28.0 %. A heat at 22.5 % Cr and 23.5 % Ni is perfectly legal under ASTM and fails EN. If your project asks for "904L to EN 1.4539", the mill certificate must show a chemistry inside both windows — check it before the plate is cut, not after.
  • Confirm the UNS number (N08904) on the certificate, together with the heat number and the delivery condition (solution annealed and pickled).
  • Copper is the grade's signature. An XRF check for Cu (1–2 %) distinguishes 904L from 254SMO and AL-6XN instantly, both of which have little or no copper. Do this on receipt — visual appearance tells you nothing.
  • Sulphur level matters for welding. European heats with S ≤ 0.010 % weld more cleanly than ASTM-level 0.035 % material; for shop-fabricated pressure equipment it is worth specifying.
  • Do not accept 904L as a substitute for 254SMO (or vice versa) without a corrosion review. They are different alloys with different jobs: PREN 35 vs 43, copper-bearing vs copper-poor, and a price difference of 30–40 % in favour of 904L.
  • Lead time: 904L is a stocked grade in most service-centre ranges — plate 0.5–50 mm, seamless tube and pipe, bar. Expect 1–3 weeks for standard sizes and 6–10 weeks for mill-rolled heavy plate or special tube sizes.

Buying 904L from Hangbo

We supply 904L (UNS N08904 / EN 1.4539) as plate and sheet from 0.5 to 50 mm, seamless and welded pipe and tube, round bar from 8 mm, and formed components such as bellows blanks and dished heads. Each shipment carries an EN 10204 3.1 certificate with the full heat analysis — including copper, which is the element that identifies this grade — and we PMI-verify before packing. If your specification is dual-certified ASTM plus EN, we check the narrower European window against the actual heat before the material leaves the mill. Tell us the acid, the concentration, the temperature and the chloride level, and we will confirm whether 904L is right or whether 254SMO, Alloy 20 or a nickel alloy is the better answer for that duty.

Frequently asked questions

Is 904L magnetic?

No. 904L is fully austenitic and stays essentially non-magnetic in the annealed, cold-worked and welded conditions — one of the few highly alloyed stainless grades where that holds true. A strong magnet response would suggest you have received a different grade, most likely a duplex or a 400-series steel.

Can 904L be used in seawater?

At ambient temperature and low velocity, yes — it is used for marine hardware and ambient seawater lines. It is not suitable for warm chlorinated seawater: with a PREN of about 35, its critical crevice temperature is only around 30–40 °C, so gasketed and deposited areas will crevice-corrode. For sea water above ~40 °C specify 254SMO (PREN 43) or a super duplex grade.

What is the maximum service temperature of 904L?

About 400 °C, and ASME Section VIII lists allowable stresses only to roughly 371 °C. Between 400 and 600 °C sigma phase precipitates quickly, reducing toughness and corrosion resistance. 904L is a corrosion grade, not a heat-resistant grade — for high-temperature duty use 309S/310S, 800H or a nickel alloy.

904L vs 316L — what am I actually paying for?

Roughly twice the nickel, twice the molybdenum and 1–2 % copper, which buys you sulphuric acid resistance across the full concentration range, a PREN of 35 instead of 25, and much better chloride SCC resistance. The price is typically 2.5–3.5× 316L per kilogram. In dilute sulphuric acid service the service life difference is not incremental — 316L fails in months where 904L lasts decades.

Which filler metal for welding 904L?

ER385 for TIG and MIG, or E385-15/-16/-17 covered electrodes. Never 308L or 316L: the weld metal would be significantly under-alloyed in Ni, Mo and Cu, would pit preferentially and would be prone to solidification cracking. For critical corrosion service an overmatched nickel filler such as ERNiCrMo-3 can be specified, but ER385 is the standard matching choice.

Is 904L the same as 1.4539?

Almost, but not exactly. Both refer to UNS N08904 chemistry, but EN 1.4539 restricts Cr to 19.0–21.0 % and Ni to 24.0–26.0 %, while ASTM allows Cr 19.0–23.0 % and Ni 23.0–28.0 %. A dual-certified item must satisfy both, and the EN window is the binding one. Always state which specification governs when you place the order.

Need 904L (UNS N08904)?

Send us your drawing or specification for a quotation — we reply within one business day.

Request a quote