[email protected] WhatsApp +86 159 0085 2030 Qingpu, Shanghai Reply within 1 business day

317L (UNS S31703): composition, properties and applications

317L is what you buy when 316L is *almost* good enough. It keeps the same 18-8 austenitic backbone but lifts molybdenum from 2-3 % to 3-4 %, chromium from 16-18 % to 18-20 % and nickel from 10-14 % to 11-15 %, which moves the pitting resistance equivalent from roughly 25 to roughly 30. That is not enough for seawater, but it is exactly enough for bleach-plant filtrates, moderate-chloride chemical tanks and hot organic acids where 316L pits within a few years. This guide gives the numbers, the real differences against 316L and 317LMN, and the traps we see in purchase orders every week.

Stainless steel seamless tubes in warehouse

What 317L is, and what it is not

317L (UNS S31703, W.Nr 1.4438, EN X2CrNiMo18-15-4) is a low-carbon, molybdenum-rich austenitic stainless steel. Compared with 316L it carries roughly one extra percent of molybdenum, one to two extra percent of chromium and one extra percent of nickel. Those single percentage points are what turn a general-purpose 18-8 into a grade that survives chloride-bearing process streams a full notch above what 316L can take.

The "L" matters: carbon is capped at 0.030 %, which keeps chromium carbides in solution through welding and therefore removes the need for post-weld heat treatment in normal thicknesses. 317L is fully austenitic at room temperature, non-magnetic in the annealed condition, and cannot be strengthened by heat treatment — only by cold work.

What 317L is not: it is not a seawater alloy, it is not a super-austenitic, and it is not a substitute for 904L or the 6 % Mo grades in hot sulphuric acid. It sits in the middle of the ladder, and most of the value we add for customers is telling them honestly which rung they actually need.

One-line positioning: 317L is a 316L with about 5 extra PREN points. It buys you a real service-life extension in chlorides and organic acids at a premium of roughly 15-30 % over 316L — far less than jumping to 904L or 254SMO.

Chemical composition (ASTM A240)

ElementContent (wt %)What it actually does
Chromium (Cr)18.0-20.0Passive film former; sets the baseline for general corrosion and oxidation resistance. 2 points above 316L is the main reason 317L handles hotter oxidising streams.
Nickel (Ni)11.0-15.0Stabilises the austenite and raises toughness and acid resistance. The 11 % floor (vs 10 % for 316L) gives margin against delta-ferrite and sigma formation.
Molybdenum (Mo)3.0-4.0The defining element: each percent of Mo adds about 3.3 PREN points and is what resists pitting and crevice attack in chlorides.
Carbon (C)0.030 maxLow carbon prevents chromium-carbide precipitation in the weld HAZ, so no PWHT is required after welding.
Nitrogen (N)0.10 maxNot deliberately added (unlike 317LMN). Residual nitrogen from melting adds a small amount of strength and pitting resistance.
Manganese (Mn)2.00 maxDeoxidation and austenite balance; no functional role in corrosion resistance.
Silicon (Si)0.75 max (1.00 in some product specs)Deoxidation. High silicon hurts weldability and surface quality — keep it low.
Phosphorus / Sulphur0.045 / 0.030 maxResiduals; sulphur in particular drives hot cracking, so low-S is preferred for welded tube.
Iron (Fe)BalanceMatrix.

Note the overlap with 316L: ASTM allows 316L up to 3.00 % Mo and 317L from 3.00 % Mo upwards. A heat sitting exactly at 3.0 % Mo can legally be certified as either grade — see the purchasing section, because this is the single most common substitution problem with this alloy.

Mechanical properties by product form

Minimum values from the ASTM product specifications, with typical mill-certificate ranges in square brackets. 317L is supplied in the solution-annealed condition; it is not hardenable by thermal treatment.

Product / conditionYield 0.2 % (MPa)Tensile (MPa)ElongationHardness
Plate & sheet, annealed — ASTM A240≥ 205 [240-300]≥ 515 [550-650]≥ 40 % [45-55]≤ 95 HRB
Bar & rod, annealed — ASTM A276 / A479≥ 205 [240-310]≥ 515 [550-660]≥ 40 % [45-55]≤ 95 HRB (approx. 217 HB)
Seamless / welded pipe — ASTM A312 TP317L≥ 205 [235-290]≥ 515 [550-640]≥ 35 % [40-55]—
Heat-exchanger tube — ASTM A213 TP317L≥ 205≥ 515≥ 35 %≤ 95 HRB
Cold-worked (drawn tube, formed sheet)Not standardised — rises with cold reduction; 1/4 hard typically 400-550Rises with cold reductionFalls sharply (10-25 %)Rises with cold work

Design notes. The pipe specification asks for 35 % elongation against 40 % for plate — a difference that matters when you are comparing offers. Cold work is the only strengthening route, and it costs ductility and adds magnetic response; if you need strength plus corrosion resistance at temperature, that is a different alloy family (duplex or a 6 % Mo grade), not a harder 317L. 317L also has a pronounced work-hardening rate: bend radii and springback allowances should follow 316L practice or be slightly more generous.

Physical properties

PropertyValuePractical consequence
Density7.98 g/cm3 (8.00 in some tables)Weight calculations: 1 mm plate ≈ 7.98 kg/m2
Melting range≈ 1370-1400 °C (some sources up to 1421 °C)Hot working window 1150-1230 °C; never forge below ~900 °C
Thermal conductivity≈ 14.5-16.3 W/m·K at 100 °C; ≈ 21 W/m·K at 500 °CLow compared with carbon steel (≈ 45) — heat-exchanger surfaces run hotter than the tube-side fluid suggests
Specific heat≈ 500 J/kg·KThermal transient calculations
Mean expansion 20-100 °C≈ 16.0-16.5 ×10-6/KAbout 1.5× carbon steel: thermal fatigue in cyclic service is a real design issue
Mean expansion 20-300 °C≈ 17.5 ×10-6/KUse the temperature band that matches your duty, not the 20-100 °C figure
Mean expansion 20-650 °C≈ 18.5 ×10-6/K
Modulus of elasticity≈ 193-200 GPaLower than carbon steel (210): more deflection for the same section
Electrical resistivity≈ 0.74-0.79 µΩ·m at 20 °CAbout 45× copper — relevant for earthing and for resistance welding
Magnetic behaviourNon-magnetic when annealed (µ < 1.02); slight response after heavy cold workA magnet test is not a grade test

Values are typical for annealed product at room temperature; mill datasheets differ by a few percent between producers, so for critical thermal design ask for the heat-specific data sheet rather than a generic table.

Corrosion resistance: where 317L holds and where it fails

For austenitic and duplex stainless steels the usual single-number screen is the pitting resistance equivalent:

PREN = %Cr + 3.3 × %Mo + 16 × %N

For 317L at mid-range composition (19 % Cr, 3.5 % Mo, 0.05 % N) this gives about 30. For 316L (17 % Cr, 2.5 % Mo) it gives about 25, and for 904L about 35. Ranking alloys by PREN is a screen, not a design calculation — but the ordering is reliable and it explains almost every field success and failure of this grade.

  • Chloride pitting and crevice corrosion: the core competence. 317L tolerates chloride levels where 316L already pits, which is why it became the default material for pulp bleach-plant filtrates, chlorine-dioxide stage equipment and chloride-bearing scrubber liquors. It is not a seawater grade: gasketed joints and deposits in ambient seawater will still initiate crevice attack.
  • Sulphuric acid: useful only in dilute solutions at low temperature (roughly up to 5 % and near ambient). Hot or concentrated H2SO4 requires 904L, Alloy 20 or a nickel alloy — 317L will fail quickly, and no amount of extra molybdenum in this family fixes it.
  • Organic and mildly reducing acids: good in acetic, formic, citric, lactic and fatty-acid streams, including at moderate temperature. This is a large and under-appreciated part of 317L demand in chemical and food processing.
  • Nitric acid and oxidising media: good to excellent, comparable to 304L/316L; low carbon keeps welds sound in nitric service.
  • Intergranular corrosion after welding: the 0.030 % carbon cap plus a proper solution anneal gives good resistance in standard thicknesses. Heats sitting at the top of the carbon range and welded with high heat input are the exception — specify C ≤ 0.025 % if the weld will see nitric or other strongly oxidising acid.
  • Stress-corrosion cracking: the high nickel content delays chloride SCC compared with 304, but 317L is still an austenitic grade and will crack above roughly 60 °C in concentrated chlorides under stress. Insulation soaked with chloride-containing water is the classic field failure.
  • High temperature: oxidation resistance is quoted to about 870 °C in continuous service, but 317L is not a creep-resistant grade. Above roughly 550-600 °C, move to 321/347 (stabilised) or 310S; the molybdenum that helps in chlorides actually reduces high-temperature strength and stability.

Selection rule: use PREN to choose the family, then use the medium to check the corners. 317L (PREN ≈ 30) handles chlorides up to a few hundred mg/L at moderate temperature; above that go to 317LMN (≈ 35), 904L (≈ 35), 2205 duplex (≈ 35) or a 6 % Mo grade (≈ 43). In hot sulphuric acid, PREN tells you nothing — go straight to 904L, Alloy 20 or C-276.

317L against its neighbours: 316L, 317LMN, 904L, 254SMO

GradeCr / Ni / Mo / N (%)PRENWhere it winsWhere it loses
316L (S31603)16-18 / 10-14 / 2.0-3.0 / ≤0.10≈ 24-26Cheapest, universally available, fine for mild chlorides and most food/pharma dutyPits in bleach filtrates and chloride-bearing scrubber liquors
317L (S31703)18-20 / 11-15 / 3.0-4.0 / ≤0.10≈ 29-31Moderate chloride + acid; pulp & paper, chemical tanks, FGD internalsNot seawater; not hot H2SO4; not a creep grade
317LMN (S31726, 1.4439)17-20 / 13.5-17.5 / 4.0-5.0 / 0.10-0.20≈ 34-36The true step above 317L: nitrogen gives strength plus pitting resistance; common European substituteHigher price, narrower availability, more welding discipline needed
904L (N08904, 1.4539)19-23 / 23-28 / 4.0-5.0 / ≤0.10≈ 35Copper addition makes it the sulphuric-acid austenitic; also strong in phosphoric acidExpensive nickel content; sigma phase above ~400 °C
254SMO (S31254)19.5-20.5 / 17.5-18.5 / 6.0-6.5 / 0.18-0.22≈ 43Seawater, high-chloride bleach, desalination — real chloride immunity2-3× the price of 317L; not for hot concentrated acid

In practice, three questions settle it: how much chloride, at what temperature, and is the acid oxidising or reducing. Answer those and the table collapses to one row. If a customer asks for "317L but better", 317LMN is usually the honest answer before jumping to 904L.

Applications by industry

IndustryTypical 317L componentsWhy 317L specifically
Pulp & paperBleach-plant washers and filtrate piping, ClO2 stage equipment, digester flashing lines, black-liquor handling, stock chestsChloride + chlorine-dioxide + low pH; the historical home market of the grade
Chemical processingReaction vessels, storage tanks, columns and internals for acetic/formic/citric acid, heat-exchanger tubing, pump casingsOrganic acids with moderate chloride, where 316L pits at welds and heat-affected zones
Flue-gas desulphurisationAbsorber internals, mist eliminators, duct liners, spray headers (lower-chloride scrubbers)Chloride-bearing condensates at 50-80 °C; higher-chloride designs go to 2205 or AL-6XN
Refining & petrochemicalPiping and exchanger tubes in chloride-bearing process streams, tank linings, sour-water servicesBetter chloride margin than 316L without stepping into nickel alloys
Water treatmentBrackish-water piping, dosing skids, chlorination equipmentTolerates hypochlorite dosing where 316L stress-corrosions
Food & pharmaceuticalTanks, piping and fittings in high-chloride cleaning regimes (CIP with hypochlorite)Cleanability of 316L with better resistance to chloride cleaning chemicals
Marine (non-immersed)Splash-zone brackets, fasteners, deck fittings above the waterlineOnly for atmospheric/splash duty — not for immersion

Standards and product forms we supply

  • Plate, sheet, strip: ASTM A240 / ASME SA-240; EN 10088-2 (1.4438)
  • Bar, rod, wire rod: ASTM A276, ASTM A479 (pressure-service bar)
  • Seamless and welded pipe: ASTM A312 TP317L / ASME SA-312
  • Heat-exchanger and condenser tube: ASTM A213 TP317L; welded tube A249 / A269 / A270
  • Forgings, flanges, fittings: ASTM A182 F317L, A403 WP317L
  • Weld consumables: ER317L (AWS A5.9), E317L-16/-17 (AWS A5.4); ERNiCrMo-3 for dissimilar joints to higher alloys
  • Supply condition: solution annealed and pickled / descaled; EN 10204 3.1 mill certificates with PMI as standard
  • Size range from stock: plate 0.5-60 mm, bar 6-250 mm, seamless pipe 6-630 mm OD, welded pipe to 2,000 mm OD

Note on European supply: 1.4438 (X2CrNiMo18-15-4) is the direct EN equivalent and is usually dual-certified. 1.4439 is not 317L — it is 317LMN with 4.0-5.0 % Mo and deliberate nitrogen, and it cannot be substituted one-for-one in a pressure design without re-checking the allowable stresses.

Fabrication, welding and heat treatment

  • Solution annealing: 1040-1120 °C, then rapid cooling (water or forced air). This is the supply condition and the only way to restore full corrosion resistance after hot forming or severe cold work.
  • Hot working: 1150-1230 °C, finishing above ~900 °C, followed by water quenching. Soaking in the 600-900 °C band precipitates sigma phase and carbides and will show up later as intergranular attack.
  • Cold forming: similar to 316L but with higher springback and faster work hardening; anneal between severe drawing passes. Deep-drawn parts should be re-annealed before service in corrosive media.
  • Machining: gummy and work-hardening; sharp positive-rake carbide inserts, heavy feeds, no dwelling in the cut. Do not let the tool rub — that is what work-hardens the surface.
  • Welding process: TIG, MIG, SMAW, SAW and orbital welding all work. No preheat. Keep interpass temperature below 150 °C and use low heat input, because 317L is fully austenitic and therefore more prone to solidification cracking than 316L.
  • Filler metal: ER317L for matching joints. For joints to 904L, 254SMO or nickel alloys use ERNiCrMo-3. Never use 308L or 316L filler on 317L — the weld becomes the weakest link and will pit first.
  • Post-weld: no PWHT is required to restore corrosion resistance, because the carbon is already low. A stress-relief anneal (around 400-450 °C) is sometimes used on cold-worked parts, but never in the 600-900 °C sensitisation band.
  • Cleaning: pickling and passivating after welding is standard practice and is what actually restores the passive film. Remove all iron contamination — carbon-steel grinding dust is the second most common cause of pitting complaints on this grade.

Welding rule of thumb: low heat input, low interpass temperature, matching ER317L filler, and pickle afterwards. A 317L weld that is not pickled will pit in the HAZ long before the base metal does.

Buying 317L: the four checks that prevent a wrong shipment

  1. Verify molybdenum, not the name. 316L is permitted up to 3.00 % Mo and 317L starts at 3.00 %. A heat at exactly 3.0 % Mo satisfies both. If your design depends on 317L performance, specify Mo ≥ 3.2 % or state a minimum PREN in the purchase order.
  2. Confirm carbon is actually 0.030 max. "317" without the L is 0.08 % carbon and will sensitise in the HAZ. The difference is invisible on a PMI gun — carbon cannot be measured by handheld XRF — so it must come from the mill certificate or a combustion analysis.
  3. Check the elongation figure against the product form. Plate is 40 %, pipe and tube 35 %. An offer quoting 40 % elongation on seamless pipe has probably copied a plate certificate.
  4. Ask for the heat number on both the plate and the filler. Mixed shipments are the norm in job-shop fabrication and traceability is what protects you if a weld pits in year two.

From our Shanghai facility we supply 317L plate, sheet, bar, seamless and welded pipe, tube, forgings and fittings, cut to size, with EN 10204 3.1 certificates, PMI on every heat and third-party inspection (SGS, BV, TUV) on request. Typical lead time is 7-15 days for stock sizes and 25-40 days for mill-roll or forged items.

Frequently asked questions

Is 317L worth the extra cost over 316L?

Only if the chloride or acid duty is what drives the choice. 317L costs roughly 15-30 % more than 316L and gives about 5 PREN points. In pulp bleach plants, hypochlorite dosing lines and chloride-bearing organic acids that premium pays for itself within one maintenance cycle. In plain cooling water or food duty, 316L is the correct and cheaper answer.

Can 317L be used in seawater?

No, not for immersion. PREN 29-31 is well below the roughly 40 needed for reliable seawater service, and gasketed or welded crevices will initiate attack. For seawater use 2205 or 2507 duplex, 254SMO, AL-6XN or a nickel alloy such as 625. 317L is acceptable only for atmospheric and splash-zone duty above the waterline.

What is the difference between 317 and 317L?

Carbon: 0.08 % max for 317 versus 0.030 % max for 317L. 317L is the standard supply grade today; plain 317 is rarely stocked and should not be substituted where welded equipment sees corrosive service. Handheld PMI cannot tell them apart because it cannot measure carbon — always read the certificate.

Does 317L need post-weld heat treatment?

No. The low carbon content means no chromium-carbide precipitation in the heat-affected zone, so corrosion resistance is retained without PWHT. What is required is weld cleaning: pickling and passivating to restore the passive film, plus removal of all iron contamination.

Is 317L magnetic?

In the annealed condition it is essentially non-magnetic, with permeability below 1.02. Heavy cold work (cold-drawn tube, formed sheet) produces a slight magnetic response, which is normal and does not mean the grade is wrong.

What is the maximum service temperature of 317L?

Oxidation resistance is quoted to about 870 &deg;C in continuous service, but that is not a structural rating. 317L is not a creep-resistant grade, and above roughly 550-600 &deg;C the stabilised grades (321, 347) or 310S are the correct choice. In pressure design, use the ASME allowable stress tables for the actual temperature rather than a generic maximum.

Need 317L (UNS S31703)?

Send us your drawing or specification for a quotation — we reply within one business day.

Request a quote