321 / 347 / 321H / 347H: stabilised stainless steels for 425-900 °C service

321 and 347 exist for one reason: to survive the 425-900 °C band where ordinary 304 precipitates chromium carbides and starts to fall apart from the inside. 321 ties up carbon with titanium, 347 ties it up with niobium plus tantalum, and both keep chromium in solution so that welded equipment can be put into hot service without a post-weld anneal. The two grades are chemically almost twins and commercially very different — 347 is the better welder, 321 is the cheaper and more formable one, and choosing wrongly costs either money or a weld. This guide sets out the numbers, the stabilisation ratios that actually govern acceptance, and the decision rules we apply to refinery, power and exhaust-system enquiries.

Stainless steel seamless tubes in warehouse

Why stabilised grades exist

When an austenitic stainless steel is held or slowly cooled through roughly 425-900 °C, chromium and carbon combine as chromium-rich carbides (M23C6) along the grain boundaries. The chromium is consumed locally, the adjacent zone drops below the ~12 % needed for a passive film, and the material becomes sensitive to intergranular corrosion. This is sensitisation, and in welded equipment it happens in the heat-affected zone during the weld thermal cycle itself.

There are only three industrial answers. Reduce the carbon (the "L" grades, 304L/316L). Anneal after welding (rarely practical on a large fabrication). Or add a strong carbide former that grabs the carbon before chromium does — titanium in 321, niobium in 347. These are the stabilised grades: UNS S32100 and S34700, W.Nr 1.4541 and 1.4550, with high-carbon variants 321H (S32109, 1.4878) and 347H (S34709, 1.4912) for creep duty.

The consequence is a grade family that behaves like 304 in ambient corrosion but like a different material at temperature — and, importantly, that can be welded and put straight into 500-900 °C service without heat treatment. That combination is why 321 and 347 remain in every refinery and power-plant material specification written since the 1950s.

The single fact that justifies the grade: between 425 and 900 °C, unstabilised 304/304L will sensitise and can fail by intergranular attack; 321 and 347 will not. Below 425 °C, 304L does the same job for less money.

Chemical composition: 321, 321H, 347, 347H

Element321 (S32100)321H (S32109)347 (S34700)347H (S34709)Role
Carbon0.08 max0.04-0.100.08 max0.04-0.10Higher C in the H grades raises creep strength; it is also why the stabiliser ratio tightens
Chromium17.0-19.017.0-19.017.0-19.017.0-19.0Passive film and oxidation resistance
Nickel9.0-12.09.0-12.09.0-13.09.0-13.0Austenite stability, toughness, delayed SCC
Titanium5×(C+N) min, 0.70 max4×(C+N) min, 0.70 max——Carbide former; the ratio, not the absolute value, is the acceptance criterion
Niobium + Tantalum——10×C min, 1.00 max8×C min, 1.00 maxStronger carbide former than Ti and it survives the welding arc
Manganese2.00 max2.00 max2.00 max2.00 maxDeoxidation, austenite balance
Silicon0.75 max0.75 max0.75 max0.75 maxDeoxidation
Phosphorus / Sulphur0.045 / 0.030 max0.045 / 0.030 max0.045 / 0.030 max0.045 / 0.030 maxResiduals; low S for weldability
IronBalanceBalanceBalanceBalanceMatrix

Two specification details are routinely missed. First, the stabilisation requirement is a ratio: a 321 heat at 0.06 % C needs at least 0.30 % Ti (5 × C, ignoring the small nitrogen term), and a 347 heat at 0.06 % C needs at least 0.60 % Nb+Ta. A certificate showing "Ti 0.25 %" against 0.06 % C fails that ratio even though it is full of titanium. Second, 321H carries an additional requirement of ASTM grain size No. 7 or coarser, which is what delivers the elevated-temperature strength; a fine-grained 321H should be queried.

Never accept "Ti: present" or "Nb: present" as evidence of stabilisation. Recalculate the ratio from the certificate: Ti ≥ 5 × C for 321, ≥ 4 × C for 321H, Nb+Ta ≥ 10 × C for 347, ≥ 8 × C for 347H.

Mechanical properties by grade and form

Room-temperature minima in the annealed condition, with typical mill ranges in square brackets. All four grades share the same 515/205 MPa floor — the H grades earn their keep above 540 °C, not at room temperature.

Grade / formYield 0.2 % (MPa)Tensile (MPa)ElongationHardness
321 plate & sheet, annealed — A240≥ 205 [230-290]≥ 515 [550-640]≥ 40 % [45-58]≤ 95 HRB (≈ 217 HB)
321H plate & sheet, annealed — A240≥ 205 [240-300]≥ 515 [550-650]≥ 40 % [40-50]≤ 95 HRB
347 plate & sheet, annealed — A240≥ 205 [230-290]≥ 515 [550-650]≥ 40 % [45-55]≤ 92 HRB (≈ 201 HB)
347H plate & sheet, annealed — A240≥ 205 [240-310]≥ 515 [555-660]≥ 40 % [40-50]≤ 92 HRB
Bar, annealed — A276 / A479≥ 205≥ 515≥ 40 %≤ 95 HRB
Seamless pipe / tube — A312, A213≥ 205≥ 515≥ 35 %—
Cold-worked (drawn tube, formed strip)Not standardised; rises with cold reductionRises with cold reductionFalls with cold reductionRises

At temperature the picture changes. The stabilised grades retain higher strength than 304 above roughly 540 °C, and the difference between 347 and 347H becomes significant in the creep regime — ASME allowable stresses for 347H reflect that higher strength, which is why 347H is the default for superheater and reformer duty. Do not extrapolate room-temperature values: for design above 425 °C use the ASME BPVC Section II Part D tables for the specific grade, product form and temperature.

Physical properties (321 vs 347)

The two grades are near-identical physically; the small differences come from titanium versus niobium atomic weight. Values are typical for annealed material.

Property321347Note
Density7.92 g/cm3 (some tables 8.03)7.96 g/cm3Grade-data sheets in circulation often round both to 7.90 — acceptable for estimating, not for weight-critical fabrication
Melting range≈ 1398-1446 °C≈ 1398-1446 °CPractically identical; drives the 1150-1200 °C hot-working window
Thermal conductivity≈ 16.1 W/m·K at 100 °C; ≈ 22.2 at 500 °C≈ 16.1 W/m·K at 100 °C; ≈ 22.2 at 500 °CAbout one third of carbon steel — thermal gradients across walls are steep
Specific heat (0-100 °C)≈ 500 J/kg·K≈ 500 J/kg·KSame basis for transient calculations
Mean expansion 20-100 °C≈ 16.6 ×10-6/K≈ 16.6 ×10-6/KUse the band that matches the duty. Expansion roughly doubles the carbon-steel value — design expansion joints accordingly
Mean expansion 20-315 °C≈ 17.2 ×10-6/K≈ 17.2 ×10-6/K
Mean expansion 20-538 °C≈ 18.6 ×10-6/K≈ 18.6 ×10-6/K
Modulus of elasticity≈ 193 GPa≈ 193 GPaFalls steeply with temperature; check the value at design temperature
Electrical resistivity (20 °C)≈ 0.72 µΩ·m≈ 0.73 µΩ·mRelevant for resistance welding and electrical heating elements
Magnetic behaviourNon-magnetic annealed; µ < 1.02 at 200 HNon-magnetic annealed; µ < 1.02 at 200 HWeld ferrite, if any, raises permeability locally

Because the physical properties are identical, 321 and 347 are interchangeable in thermal-stress and expansion-joint calculations. The choice between them is driven by welding, corrosion in specific media, and availability — not by physics.

Heat resistance, sensitisation and the 425-900 °C band

Three separate phenomena are often lumped together as "high-temperature behaviour". They need to be checked separately.

  • Oxidation (scaling). 321 and 347 resist oxidation to about 925 °C in continuous service and about 900 °C intermittently. Above roughly 900 °C, chromium depletion at the surface becomes rapid and 310S or a nickel alloy is the right move. Cyclic service is more severe than continuous because the oxide spalls and re-forms.
  • Sensitisation (intergranular corrosion). This is the reason the grades exist. In the 425-900 °C band, chromium carbides form within minutes to hours in unstabilised grades. In 321 the titanium carbides form preferentially and in 347 the niobium carbides do, so chromium stays in solution. The practical statement: 321 and 347 can be welded and placed directly into 425-900 °C service without a post-weld anneal, provided the stabilisation ratio is met.
  • Creep and stress rupture. A different mechanism and a different limitation. Standard 321/347 are creep-limited well below their oxidation limit; the H grades (0.04-0.10 % C) carry the higher allowable stresses above roughly 540 °C. For superheater tubing, reformer internals and other long-life creep duty, always specify 321H or 347H rather than relying on the low-carbon grade.
  • Sigma phase. Prolonged exposure in the 600-900 °C range also precipitates sigma in these grades, reducing toughness. It matters for thick sections and for cyclic shutdowns, less for thin-wall tubing.

The 425-900 °C band is a materials-selection gate, not a nuance. Below 425 °C use 304L/316L. Between 425 and 900 °C use 321 or 347 (or the H grades for creep duty). Above ~900 °C move to 310S or a nickel alloy. Equipment that crosses the band during welding is exactly why stabilised grades were invented.

Aqueous corrosion: what stabilisation does and does not buy

In the annealed condition, 321 and 347 resist general corrosion about as well as 304. Stabilisation is not a corrosion upgrade in the way molybdenum is; it protects one specific failure mode, intergranular attack, and mostly after welding. Both grades contain no molybdenum, which gives them a PREN of only about 18.

Environment321347Comment
Intergranular corrosion after welding (e.g. ASTM A262 Practice E)GoodBetter347 is more tolerant of off-ratio heats and of heavy sections
Polythionic acid (refinery shutdowns, sulphidic scale + moisture + oxygen)AcceptableExcellent347 is the refinery standard for this failure mode; soda-ash neutralisation is still required
Nitric acid, oxidising mediaExcellentExcellentLow carbon plus stabilisation keeps welds sound
Dilute sulphuric / phosphoric acidFairFairUse 904L or Alloy 20 for anything beyond trace concentration
Chloride pitting and crevicePoor (PREN ≈ 18)Poor (PREN ≈ 18)Neutral chlorides are the wrong duty for these grades — go to 2205, 317L or a 6 % Mo grade
Chloride stress-corrosion crackingPoor above ≈ 60 °CPoor above ≈ 60 °CSame limitation as 304; duplex or high-nickel alloys are the answer
High-temperature sulphidation / carburisationModerateModerateBetter than 304, far below nickel alloys

One practical point that catches fabricators: 321 does not polish well. Titanium forms stringers and inclusions during melting, and these tear at the surface during polishing, leaving a speckled finish. For decorative or hygienic polished surfaces, 304/316L or 347 are preferred over 321.

321 or 347? The decision matrix

Criterion321 wins347 wins
Welding extentLight welding, or formed components joined at a few seamsHeavy welded assemblies, thick sections, no post-weld anneal possible
Weld filler availability321 filler is effectively unavailable — 321 base metal is welded with ER347 anywayER347 is a stock item worldwide; the practical default filler for both grades
Service temperatureUp to about 900 °C peak, non-creep-criticalConservatively rated to about 816 °C continuous, with 347H extending creep capability above that
Refinery / polythionic acidAcceptable with neutralisationStandard choice; niobium gives markedly better resistance
Formability and costCheaper and easier to form; titanium is the lower-cost stabiliser and 321 is the higher-volume gradeDearer; niobium-bearing heats cost more and availability is narrower in thin sheet
Surface finishPoor polishing behaviour — avoid decorative useAccepts a normal polished finish
Cyclic thermal fatigue (exhaust systems)Often preferred: better formability, slightly lower density, adequate at 400-750 °CBetter for steady high-temperature service than for vibration-fatigue duty

Heuristic we apply to enquiries: exhaust and thermal-oxidiser work at 400-800 °C with light welding → 321. Refinery, petrochemical and heavy welded pressure equipment at 427-816 °C → 347 (347H for creep duty). If the item is a pressure vessel and the temperature exceeds 540 °C, specify the H grade and verify code acceptance first.

Code caveat worth checking before you commit: some mill datasheets note that 321H is not listed for ASME Section VIII Div. 1 construction (347H is), and that 321H is limited to 427 °C in Section III nuclear applications. If the vessel is code-stamped, confirm the grade is in the applicable ASME table before releasing the order.

Applications by industry

IndustryTypical componentsGrade usually specified
AerospaceExhaust manifolds and cones, afterburner and tailpipe components, bellows, heat shields321 (formability, cyclic 400-750 °C)
Oil refining / petrochemicalCatalytic reformer internals, exchanger tubes, transfer line piping, reactor internals, flare tips347 / 347H (polythionic acid, creep)
Power generationSuperheater and reheater tube supports, boiler tube hangers, soot-blower parts, expansion joints347H / 321H
Chemical processingExpansion joints, bellows, thermal-oxidiser shells, nitric acid equipment, catalyst beds321 (light welding), 347 (welded)
AutomotiveExhaust systems, catalytic converter shells, flex couplings, turbo downpipes321 (also 409/441 at lower duty)
Heat treatment & furnacesRetorts, muffles, fans, radiant tubes, conveyor parts below ~900 °C321 / 347, 310S above 900 °C
NuclearPiping, surge lines, core support structures (grade-specific code limits apply)347
Pulp & paper / foodDigester piping in elevated-temperature zones, steam-side equipment321 / 347

Standards and product forms

  • Plate, sheet, strip: ASTM A240 / ASME SA-240 (321, 321H, 347, 347H); EN 10088-2 (1.4541, 1.4550)
  • Aerospace sheet and strip: AMS 5510 (321), AMS 5512 (347)
  • Bar and rod: ASTM A276, ASTM A479
  • Seamless and welded pipe: ASTM A312 TP321 / TP321H / TP347 / TP347H
  • Heat-exchanger and condenser tube: ASTM A213; welded tube A249 / A269
  • Forgings, flanges, fittings: ASTM A182 F321 / F347, A403 WP321 / WP347
  • Weld consumables: ER347 (AWS A5.9), E347-16/-17 (AWS A5.4); ER347 is the standard filler for both 321 and 347 base metal
  • European equivalents: 1.4541 = 321, 1.4878 = 321H, 1.4550 = 347, 1.4912 = 347H — dual certification is common but check the carbon range matches the grade ordered
  • Supply condition: solution annealed 950-1120 °C, rapid cooled, pickled; EN 10204 3.1 certificates with PMI and stabiliser ratio verification

Fabrication, welding and heat treatment

  • Solution annealing: 950-1120 °C followed by rapid cooling. This dissolves carbides and is the supply condition.
  • Stabilising anneal: 870-900 °C, one hour per 25 mm of thickness, air cooled. Recommended for severe service above 425 °C and for material annealed at the top of the range, because it lets the stabiliser carbides form before service does it for you.
  • Stress relief: about 700 °C for one to two hours if required for dimensional stability. Never stress-relieve in the 425-900 °C sensitisation band without a stabilising treatment.
  • Filler metal: ER347 (or E347 covered electrodes) for both 321 and 347 base metal. This is not a shortcut — titanium is oxidised and lost in the weld pool, so a "matching" 321 filler would leave the weld depleted of stabiliser. ER347 also covers 321-to-347 and 321-to-carbon-steel dissimilar joints.
  • Heat input: no preheat. Keep interpass temperature below 150 °C, use stringer beads rather than wide weaves, and purge the root on tube and pipe work. Both grades are fully austenitic and prone to solidification cracking if heat input is excessive.
  • Post-weld heat treatment: not required to restore corrosion resistance in either grade. Required in some code cases: ASME VIII Div. 1 calls for PWHT on thick-wall vessels above 38 mm (with exceptions), and PWHT is specified for caustic and polythionic-acid service regardless of thickness.
  • Pickling and passivation: still necessary after welding. Stabilisation prevents chromium depletion from carbides; it does nothing about heat tint, iron contamination or a chromium-depleted as-welded surface.
  • Machining and forming: both grades machine like 304 with a strong tendency to work-harden — sharp tools, positive rake, no dwell. 321's titanium stringers affect surface finish; 347 forms and polishes more predictably.

The most common welding error with these grades is ordering ER321 filler. There is essentially no commercial ER321 supply, and using it would be wrong anyway: 321 base metal is welded with ER347, and that is what the procedure qualification should say.

Buying 321/347: what to put on the purchase order

  1. State the grade and the H-variant explicitly. "321" and "321H" differ only in carbon (0.08 max vs 0.04-0.10) — and carbon is invisible to a handheld XRF gun. If creep duty matters, the H grade must be on the order, on the certificate and on the heat tag.
  2. Require the stabiliser ratio on the certificate. Ti ≥ 5 × C (321), 4 × C (321H), Nb+Ta ≥ 10 × C (347), 8 × C (347H). Recompute it yourself; off-ratio heats are the most frequent non-conformity we see on incoming inspection.
  3. Specify grain size for 321H. ASTM No. 7 or coarser is part of the specification and is what delivers elevated-temperature strength.
  4. Check the product form against the elongation figure. Plate is 40 %, pipe and tube 35 %. A pipe certificate quoting 40 % deserves a question.
  5. Ask whether the item is dual-certified. 1.4541/1.4550 heats are often certified to both EN and ASTM; the carbon ranges are compatible, but 1.4878 (321H) and 1.4912 (347H) must be checked against the ASTM H-grade limits.
  6. For refinery duty, add the corrosion test. ASTM A262 Practice E (intergranular corrosion) is the standard acceptance test for stabilised grades in polythionic-acid service and is cheap insurance.

Hangbo supplies 321, 321H, 347 and 347H as plate, sheet, bar, seamless and welded pipe, heat-exchanger tube, forgings, flanges and fittings, cut and machined to drawing. Certificates are EN 10204 3.1 with heat-number traceability, PMI on every item and stabiliser-ratio verification before dispatch; third-party inspection (SGS, BV, TUV) on request. Stock sizes usually ship in 7-15 days, mill-roll and forged items in 25-45 days.

Frequently asked questions

Should I choose 321 or 347?

If the equipment is heavily welded, thick-sectioned, or in refinery/polythionic-acid service, choose 347 (347H for creep duty). If it is formed and lightly welded, running to about 800-900 °C, and cost or formability matter — exhaust systems, thermal oxidisers, bellows — 321 is the better value. Note that 347 is the filler for both, so 347 base metal never creates a consumable problem.

Why is 321 welded with ER347 filler instead of a matching 321 filler?

Titanium is a strong oxide former and is largely lost to the slag and atmosphere in the welding arc, so a 321 weld deposit would not be reliably stabilised. Niobium transfers across the arc much more efficiently, which is why ER347 is the AWS-standard match for 321 base metal. ER321 is essentially not commercially available.

Do 321 and 347 need post-weld heat treatment?

No, not to restore corrosion resistance — that is the whole point of stabilisation. PWHT may still be required for other reasons: ASME VIII Div. 1 for thick-wall vessels above 38 mm with certain exceptions, caustic service, polythionic-acid service, or dimensional stability. A stabilising anneal at 870-900 °C is sometimes specified for severe high-temperature duty.

What does the "H" in 321H and 347H mean?

High carbon: 0.04-0.10 % versus 0.08 % max for the standard grades. The higher carbon raises creep and stress-rupture strength above roughly 540 °C, which is why superheater tubing and reformer internals are specified as 347H. The trade-off is that the stabiliser ratio requirement tightens (4 × C for 321H, 8 × C for 347H) and carbon cannot be verified by handheld PMI.

Are 321 and 347 suitable for chloride service?

No. Both contain no molybdenum, giving a PREN of only about 18, and they pit in warm chloride solutions much like 304. They also stress-corrosion crack above roughly 60 °C in concentrated chlorides. For chloride duty use 316L, 317L, 2205 duplex or a 6 % Mo grade, depending on severity.

321 versus 304L — when is the extra cost justified?

When the welded equipment will operate between 425 and 900 °C, or when it will be stress-relieved after welding. 304L can sensitise in that band and, being low carbon, has lower hot strength above about 500 °C. Below 425 °C in the annealed condition, 304L performs the same job for less money and is more readily available in every product form.

Need 321 / 347 (stabilised stainless)?

Send us your drawing or specification for a quotation — we reply within one business day.

Request a quote