Zirconium 702 (UNS R60702): composition, properties and applications

Zirconium 702 (UNS R60702) is commercially pure zirconium, and it is the alloy you reach for when the medium defeats everything else: hydrochloric acid at all concentrations up to boiling point, hot organic acids such as acetic and formic acid, and urea plant environments where even C-276 is marginal. It is roughly 25 % lighter than 316L stainless, it is nearly transparent to thermal neutrons, and its corrosion behaviour is the mirror image of titanium's — superb in reducing acids, destroyed by oxidising ions. This guide collects the verified ASTM numbers and the selection rules we apply when quoting Zr 702 plate, bar, tube and forgings.

What Zirconium 702 is — in one paragraph

Zirconium 702 (UNS R60702) is unalloyed zirconium with a minimum 99.2 % Zr+Hf and up to 4.5 % hafnium. It owes its extraordinary acid resistance to a dense, tightly adherent ZrO₂ passive film that repairs itself instantly — provided the environment contains no aggressive oxidising species. Its passive chemistry makes it the reference metal for reducing media: hydrochloric, sulfuric (mid-range), acetic, formic and lactic acids, plus hot alkalis and urea synthesis environments. Unlike most exotic metals, it is also easy on weight (6.51 g/cm³, about 25 % lighter than stainless steel) and reasonably ductile, so it fabricates like a metal rather than like a refractory.

Chemical composition (ASTM B550 / B551, UNS R60702)

ElementContent (wt %)Why it matters
Zirconium + Hafnium (Zr+Hf)99.2 minCommercially pure zirconium — the basis of the passive film and of the acid resistance
Hafnium (Hf)4.5 maxChemically almost identical to Zr; for corrosion duty it is harmless (it matters only in nuclear fuel-clad grades, where Hf must be stripped out)
Iron + Chromium (Fe+Cr)0.20 maxTrace residuals — also the reason dedicated tooling is required in fabrication (see welding section)
Oxygen (O)0.16 maxInterstitial strengthener — this is what gives CP zirconium its strength band
Carbon (C)0.05 maxInterstitial control
Nitrogen (N)0.025 maxToo much N degrades corrosion resistance; tightly limited
Hydrogen (H)0.005 maxHydrogen is zirconium's enemy — hydride precipitation embrittles the metal (see corrosion section)

Mechanical properties

Minimum values in the annealed condition, cross-checked against the governing ASTM product specifications:

Product / specificationYield strength (0.2 %)Tensile strengthElongation
Sheet & plate — ASTM B551, annealed≥ 207 MPa≥ 379 MPa (55 ksi)≥ 16 %
Bar & wire — ASTM B550, annealed≥ 205 MPa (30 ksi)≥ 380 MPa (55 ksi)≥ 16 %
Forgings — ASTM B493, annealed≈ 207 MPa≈ 379 MPa≈ 16 %
Typical mill values (annealed)[240–310][430–470][18–24]

Procurement trap worth knowing: some supplier tables list "≥ 415 MPa UTS / ≥ 240 MPa YS" for R60702 — those are actually the ASTM B550 values for Zr 704 (R60704), the Zr-Sn grade. If your certificate shows 415/240, check the UNS number and the standard on the MTC before accepting the heat.

Zirconium loses strength gently with temperature: at 300 °C the annealed alloy still retains roughly two-thirds of its room-temperature tensile strength, which is why 702 equipment routinely runs hot in acetic-acid service.

Physical properties

PropertyValue
Density6.51 g/cm³ (vs 7.98 for 316L — ~25 % lighter)
Melting point≈ 1,852 °C (sources 1,850–1,855 °C)
Thermal conductivity (RT)≈ 22 W/m·K (better than 316L ≈ 15, better than titanium ≈ 16.4)
Specific heat≈ 270–280 J/kg·K
Thermal expansion (20–100 °C)≈ 5.5–5.9 ×10⁻⁶ /K — about one third of stainless steel; generous expansion loops are rarely needed
Modulus of elasticity≈ 97–99 GPa (one source lists 88 GPa; mill data usually 97–99)
Electrical resistivity≈ 40 µΩ·cm
Magnetic behaviourNon-magnetic (paramagnetic); thermal neutron absorption cross-section ≈ 0.18 barns — the lowest of any common structural metal

Corrosion resistance — where 702 wins and where it must never be used

  • Hydrochloric acid: the headline application. Zr 702 handles HCl at every concentration, up to and above the boiling point, provided the acid is free of oxidising ions — a duty where titanium fails immediately and C-276 is usable but expensive.
  • Organic acids: outstanding in acetic, formic and lactic acid at process temperatures, including the oxygen-bearing and dilute sulphuric traces typical of acetic-acid plant circuits.
  • Urea and UAN: resists hot ammonium carbamate in urea strippers and high-pressure urea equipment far better than urea-grade stainless steels — this is the classic Zr 702 duty.
  • Strong alkalis: excellent across the full concentration range, including caustic at elevated temperature where most nickel alloys are merely acceptable.
  • Hard no-go list: hydrofluoric acid and fluorides; HCl containing ferric (Fe³⁺) or cupric (Cu²⁺) ions; wet chlorine; sulfuric acid above about 70 %; aqua regia. Any oxidising species destroys the passive film faster than it can re-form.

Selection rule: zirconium and titanium are mirror images. Titanium rules oxidising media (seawater, wet chlorine, nitric acid); zirconium rules reducing media (HCl, acetic/formic acid, urea). The most common field failure of Zr 702 is not general corrosion but hydrogen embrittlement — hydrogen uptake from galvanic coupling to less noble metals, misplaced cathodic protection, or hot reducing acid — so design against hydrogen pickup, not just wall loss.

Typical applications

IndustryTypical Zr 702 components
Acetic acid / PTAReactors, columns, heat-exchanger tubing, pump internals handling hot acetic and formic acid
Fertilizer / ureaUrea stripper linings, high-pressure carbamate equipment, UAN service
HCl / chlor-alkaliHCl coolers, absorbers, transfer lines (oxidiser-free duty)
Pharmaceutical / fine chemicalsProcess vessels and linings where product purity and acid duty overlap
NuclearFuel cladding and structural components — 0.18 barn neutron cross-section (Hf-controlled grades)
Pressure equipmentExplosion-clad plate (Zr on steel) for tubesheets and vessel shells, rupture discs, flange facings, loose-lined nozzles

Standards and product forms we supply

  • Sheet / strip / plate: ASTM B551 / ASME SB551
  • Bar & wire: ASTM B550 / ASME SB550
  • Seamless & welded tube: ASTM B523 / ASME SB523
  • Pipe: ASTM B658 / ASME SB658
  • Forgings & billet: ASTM B493 / ASME SB493
  • Weld filler: R60702-grade zirconium welding wire, matched to the parent metal
  • Forged rings, discs, blocks and machined parts: supplied to drawing with EN 10204 3.1 certificates

Fabrication, welding and buying notes

  • Welding: GTAW only, with full inert-gas shielding — torch gas plus trailing shield plus root purge, because zirconium reacts with oxygen and nitrogen above about 400 °C. Back-purging is not optional; contaminated welds show up later as brittle, discoloured joints.
  • Iron contamination is a real failure cause: embedded steel particles from carbon-steel brushes, grinding wheels or shared tooling become initiation sites in acid service. Dedicated stainless or carbide tooling and a segregated fabrication area are standard practice for zirconium work.
  • Fire safety: fine zirconium swarf and grinding dust are pyrophoric. Keep chips wet, collect them, and never let dust accumulate near ignition sources.
  • Forming: 702 forms cold or warm, but springs back noticeably more than steel — allow for overbending and re-checking.
  • Buying: always specify UNS number + product standard + condition. Because Zr 702, 704 and 705 share datasheet space on supplier sites, the UNS number on the purchase order (and the MTC) is your only real protection against substitution.

Frequently asked questions

Is Zirconium 702 magnetic?

No. Zirconium is paramagnetic and 702 is effectively non-magnetic at any condition, with negligible neutron absorption (≈0.18 barns) — one reason it is the standard structural metal inside nuclear reactors.

Zr 702 vs Titanium Gr.2 — which do I need?

They are near mirror images. Zr 702 wins in reducing acids (HCl, acetic, formic) and urea service; Gr.2 wins in oxidising media — seawater, wet chlorine, nitric acid. Putting Zr 702 into chloride-containing seawater duty, or Gr.2 into hot HCl, are the two classic and very expensive specification mistakes.

Why does 702 contain up to 4.5 % hafnium?

Hafnium always accompanies zirconium in the ore and is chemically so similar that separating it is costly. For corrosion duty Hf is harmless. Only nuclear fuel-clad material requires Hf removal, which is why 'nuclear grade' and 'chemical grade' zirconium are priced differently.

What temperature can Zr 702 equipment run at?

About 400 °C is the accepted continuous limit in corrosive media. In air (no medium) zirconium begins to oxidise rapidly above roughly 500 °C, so bare 702 should not be used as hot-air furnace hardware — that is a job for nickel alloys such as Hastelloy X.

Need Zirconium 702 (UNS R60702)?

Send us your drawing or specification for a quotation — we reply within one business day.

Request a quote