[email protected] WhatsApp +86 159 0085 2030 Qingpu, Shanghai Reply within 1 business day

Inconel X-750 (UNS N07750): composition, properties and applications

Inconel X-750 is the precipitation-hardening member of the Inconel family: essentially Inconel 600 chemistry with aluminium and titanium added, so a simple ageing treatment roughly doubles the yield strength while keeping the oxidation resistance that made 600 famous. It is the go-to alloy for gas-turbine springs and bolts, high-temperature fasteners and nuclear structural hardware — anywhere a part must hold its clamping force at 500–700 °C. This guide collects the numbers and the selection rules we use when quoting X-750 bar, forgings and wire.

Machined nickel alloy forged discs

What Inconel X-750 is — in one paragraph

Inconel X-750 (UNS N07750, W.Nr 2.4669, ~NiCr15Fe7TiAl) is a nickel-chromium-iron precipitation-hardening superalloy with at least 70 % nickel, 14–17 % chromium and 2.25–2.75 % titanium. The strengthening mechanism is entirely different from solid-solution grades like 600 or 625: aluminium, titanium and a small niobium addition precipitate a fine γ′ phase (Ni₃(Al,Ti,Nb)) during ageing, which lifts the yield strength from roughly 380 MPa in the annealed state to about 720–1,000 MPa when aged. The alloy keeps the oxidation behaviour of Inconel 600, resists relaxation outstandingly well, and remains useful from cryogenic temperature up to about 700 °C in structural and spring duty.

Nominal chemical composition

ElementContent (wt %)Why it matters
Nickel (Ni)70 minBase metal: chloride-SCC immunity, creep resistance, thermal stability
Chromium (Cr)14–17Oxidation resistance to ~980 °C short-term; general corrosion barrier
Iron (Fe)5–9Cost control and processing; kept moderate to preserve γ′ response
Titanium (Ti)2.25–2.75Primary precipitation strengthener (γ′ Ni₃Ti)
Aluminium (Al)0.4–1.0Secondary γ′ former, refines and stabilises the precipitate
Niobium + Tantalum (Nb+Ta)0.7–1.2Supports creep strength and stabilises the aged structure
Carbon (C)0.08 maxLimits carbide networks in the HAZ
Manganese / Silicon / Cobalt1.0 / 0.5 / 1.0 maxDeoxidation and residual control per ASTM B637

The Ti + Al couple is what separates X-750 from its parent 600: without it there is nothing to age-harden. That is also why X-750 is ordered with an explicit heat-treatment condition on the purchase order — the same bar can vary enormously in strength depending on how it was aged.

Mechanical properties by condition

Minimum values per ASTM B637 / AMS 5667 with typical mill-certificate ranges in brackets:

ConditionYield strength (0.2 %)Tensile strengthElongation
Solution treated / annealed (typical)≈ 380 MPa [345–420]≈ 880 MPa [850–930]≥ 30 % [30–40]
Aged, fastener condition (solution + double age)≥ 725 MPa [850–1,000]≥ 1,100 MPa [1,150–1,250]≥ 18 % [18–25]

Three standard heat-treatment schedules are in common use, and the right one depends on the duty: schedule I (885 °C equalising + 705 °C/20 h + 620 °C/8 h, triple-aged) is specified for springs where maximum relaxation resistance matters; schedule II (982 °C solution + 730 °C/8 h + 620 °C/8 h) is the common fastener/structural condition; schedule III (1,093 °C solution + 730 °C/8 h + 620 °C/8 h) suits large or welded sections. Always state the schedule on the PO — a certificate that only says "X-750, aged" is not enough.

Physical properties

PropertyValue
Density8.28 g/cm³
Melting range1,393–1,427 °C
Thermal conductivity (room temp)≈ 12 W/m·K
Specific heat≈ 430 J/kg·K
Thermal expansion (20–100 °C)≈ 13.0 ×10⁻⁶ /K
Elastic modulus (room temp)≈ 214 GPa
Magnetic behaviourEssentially non-magnetic at room temperature

High-temperature and corrosion behaviour — where X-750 fits

  • Relaxation resistance: the standout property. Bolts and springs heat-treated to schedule I keep a large share of their preload after thousands of hours at 550–650 °C, which is why X-750 remains the fastener/spring standard at turbine temperatures even though newer grades exist.
  • Oxidation: good in air and combustion atmospheres to about 980 °C for short excursions; continuous structural use is normally limited to ~700 °C, above which creep life governs.
  • Corrosion: general resistance close to Inconel 600 — good in neutral salts, alkalis and many organic media. But with only 14–17 % Cr and no molybdenum, it is not a pitting-grade alloy: avoid stagnant chloride media and acids.
  • Cryogenic: retains ductility and reasonable toughness down to −250 °C, so it also appears in cryogenic hardware.

Selection rule of thumb: choose X-750 when the problem is losing bolt preload or spring force with temperature, not corrosion. If the duty is seawater or acid pitting, move to 625 or 825; if it is creep-rated pressure parts above 600 °C, Incoloy 800H is the code-grade answer.

Typical applications

IndustryTypical X-750 components
Aerospace / gas turbinesHigh-temperature springs, bolts and studs, retaining rings, wedges and structural pins up to ~700 °C
Power generationSteam-turbine internals and fasteners, generator retaining components
NuclearStructural members and core hardware in reactor internals (the material of the well-documented pressure-vessel internals programmes)
Industrial springsBelleville washers, wave springs, spring pins and bellows requiring relaxation resistance at 450–650 °C
General engineeringHot-forming dies and high-temperature jigs where age-hardened Ni-Cr-Fe is specified

Standards and product forms we supply

  • Bar / forgings / rings: ASTM B637 / ASME SB637, AMS 5667 (aged bar), AMS 5668 / 5669 / 5670
  • Plate / sheet / strip: AMS 5542
  • Wire: AMS 5698 / 5699 (spring wire)
  • European designation: W.Nr 2.4669 / NiCr15Fe7TiAl
  • Machined parts to drawing: supplied solution-treated, aged to a named schedule, with EN 10204 3.1 certificates

Welding and fabrication notes

X-750 is weldable by TIG/MIG but with one firm rule: weld it in the solution-treated condition, then age — welding aged material embrittles the HAZ. Filler metal is normally ERNiCrFe-11 (Inconel Filler Metal 69) or ENiCrFe-11, though many fabricators simply join with FM 82 when the joint is loaded thermally rather than structurally. Machining is easiest in the annealed state; hardened X-750 (30–38 HRC after ageing) machines slowly, so leave grinding stock before final heat treatment. Cold forming of spring strip is done in the annealed condition with the ageing carried out by the spring manufacturer to schedule I.

Buying X-750 from Hangbo

We supply Inconel X-750 bar, forgings, rings, sheet and spring wire, either mill-annealed or fully heat-treated to the schedule your drawing calls out. Every lot ships with EN 10204 3.1 certificates showing the actual ageing parameters, and we can supply PMI and hardness testing on request. Typical lead time: 7–15 days for stock sizes, 30–45 days for forged or machined-to-drawing parts.

Frequently asked questions

Is Inconel X-750 magnetic?

Essentially no — like most high-nickel austenitic alloys it is non-magnetic at room temperature. A weak magnetic response after heavy cold work or straining is normal and not an indication of a wrong grade.

X-750 or Inconel 718 — which for my fasteners?

718 is stronger (aged yield ≥ 1,034 MPa vs ≈ 725 MPa for X-750) and welds more easily, which is why it dominates new aerospace designs. X-750 still wins where relaxation resistance of springs and preload retention at 550–650 °C matter most, and it is frequently specified for nuclear and retrofit steam-turbine hardware.

Which heat treatment should I order?

Tell us the duty, not just the grade. Springs and preloaded bolts: schedule I (triple age, best relaxation resistance). Standard fasteners and structural parts: schedule II (982 °C solution + 730 °C + 620 °C double age). Welded or heavy sections: schedule III (1,093 °C solution + double age).

Can X-750 replace 625 in a seawater application?

No. X-750 has no molybdenum and only 14–17 % chromium, so it is not designed for pitting/crevice resistance in seawater. 625 (PREN ≈ 50) is the correct marine alloy; X-750 is for temperature-driven strength, not chloride corrosion.