[email protected] WhatsApp +86 159 0085 2030 Qingpu, Shanghai Reply within 1 business day

Nimonic 80A (UNS N07080): composition, properties and applications

Nimonic 80A is the original workhorse of the gamma-prime-strengthened nickel superalloys: a Ni-Cr-Ti-Al alloy that owes its strength to a fine dispersion of Ni₃(Al,Ti) precipitates, holds useful creep strength to about 815 °C, and has anchored gas-turbine blading, hot bolting and diesel exhaust-valve production for eight decades. This guide collects the composition limits, aged mechanical values, physical data and the purchasing rules we apply when quoting 80A bar, forgings and rings.

Stainless steel seamless tubes in warehouse

What Nimonic 80A is — in one paragraph

Nimonic 80A (UNS N07080, W.Nr 2.4952 / 2.4631) is an age-hardenable nickel-chromium alloy with roughly 18–21 % chromium and a controlled Ti + Al addition. It is not a solid-solution alloy like 600 or 625: its strength comes from heat treatment. After solution treatment around 1,080 °C and a 700–730 °C ageing cycle, a fine, uniform dispersion of gamma-prime (γ′, Ni₃(Al,Ti)) precipitates forms and gives the alloy yield strength and creep resistance far above any austenitic steel at 650–815 °C. That combination — steel-killing creep strength with plain nickel-alloy metallurgy — is why 80A remains the default choice for hot fasteners, exhaust valves and rotating blading in industrial engines, long after flashier grades have come and gone.

Nominal chemical composition

ElementContent (wt %)Why it matters
Nickel (Ni)BalanceAustenitic matrix with good high-temperature stability
Chromium (Cr)18–21Oxidation resistance and general corrosion barrier in hot gas streams
Titanium (Ti)1.8–2.7Primary gamma-prime former — the main strengthening element
Aluminium (Al)1.0–1.8Second γ′ former; tunes the precipitate chemistry and volume fraction
Iron (Fe)3.0 maxResidual only — 80A is not a Fe-bearing Incoloy-type grade
Carbon (C)0.10 maxLimited carbides for grain-boundary control without embrittlement
Silicon / Manganese1.0 max eachDeoxidation and melting-process control
Zirconium (Zr)0.15 maxGrain-boundary refinement, improves creep ductility
Boron (B)0.008 maxTrace addition that strengthens grain boundaries against creep rupture

The Ti:Al ratio is the heart of the grade. Titanium drives the γ′ volume fraction and hence the achievable yield strength; aluminium stabilises the precipitate at temperature. Heat lots with Ti or Al at the low end of the band will not reach full aged strength — which is why reputable mills test the heat-treatment response per heat, not just the chemistry.

Mechanical properties

Room-temperature values in the bar/forging condition most buyers order (solution treated + aged), with the minima commonly quoted to ASTM B637 and typical mill-certificate ranges in brackets:

ConditionYield strength (0.2 %)Tensile strengthElongation
Solution treated + aged (ASTM B637 bar/forgings)≥ 620 MPa [760–850]≥ 1,000 MPa [1,130–1,200]≥ 15 % [15–25]

Creep-rupture figures published for 80A bar give roughly 170 MPa for 1,000 h at 750 °C and about 70 MPa at 815 °C — a useful anchor when comparing bids against A286 (which loses steam well below 700 °C) or against Nimonic 90 (which carries about 200 MPa at 750 °C). Tensile strength falls from about 1,180 MPa at room temperature to roughly 600 MPa at 750 °C and 400 MPa at 815 °C in the aged condition. Elongation in the aged state is modest compared with solid-solution nickel alloys — design for stiffness and creep, not for ductility.

Physical properties

PropertyValue
Density8.19 g/cm³
Melting range≈ 1,320–1,365 °C (some mill datasheets quote 1,360–1,390 °C)
Thermal conductivity (20–100 °C)≈ 11.2–11.7 W/m·K
Specific heat≈ 440–460 J/kg·K
Thermal expansion (20–100 °C)≈ 12.7–13.0 ×10⁻⁶ /K
Modulus of elasticity (20 °C)≈ 214–222 GPa
Electrical resistivity≈ 1.24 µΩ·m
Magnetic behaviourEssentially non-magnetic in all conditions

Published modulus figures range from about 190 to 222 GPa depending on source and condition, so confirm against the governing specification before using them in design calculations. The same applies to the melting range: chemistry bands between BS, DIN and AMS specifications shift it slightly, and no value above is a design guarantee — treat them as quoting and weight-calculation data.

High-temperature performance — where 80A earns its keep

  • Creep-limited duty to 815 °C: the γ′ dispersion resists coarsening well into this band, which is why 80A holds preload as a bolt and resists valve-stem stretch where austenitic steels relax away.
  • Exhaust-valve sulfidation resistance: in marine and heavy-oil diesel engines, fuel sulphur attacks valve steels; the Ni-Cr matrix of 80A resists the resulting sulfidation far better, making it the classic exhaust-valve alloy.
  • Oxidation resistance: 18–21 % Cr forms a stable protective scale in oxidising combustion atmospheres to about 815 °C service temperature.
  • Above the limit: beyond roughly 815 °C, γ′ coarsening and declining creep rupture strength end the design life — step up to Nimonic 90 or a cast superalloy.

Selection rule of thumb: for hot bolting, valve trim and blading in the 650–815 °C band, 80A is the cost-effective γ′-hardened benchmark. Below 650 °C, A286 usually does the same job cheaper and easier to weld; above 815 °C, move to Nimonic 90 (≈ +100 °C of creep capability) or a higher-grade superalloy.

Typical applications

IndustryTypical 80A components
AerospaceTurbine blades, vanes, discs and rotor seals in older and industrial engine designs
Power generationIndustrial gas-turbine blades, discs and casing bolting in the 650–815 °C band
FastenersStuds, bolts, nuts and hex bar holding preload on turbine casings, manifold flanges and furnace equipment
Engine / automotiveDiesel and marine exhaust valves, turbocharger wheels and shafts, high-temperature springs
NuclearBoiler tube supports and internals needing long-term creep and dimensional stability under thermal cycling
ToolingDie-casting inserts and cores exposed to molten aluminium and thermal shock

Standards and product forms we supply

  • Bars, forgings and rings: ASTM B637 / ASME SB637, UNS N07080
  • Aerospace bar: AMS 5666; forging stock: AMS 5702
  • European equivalents: W.Nr 2.4952 / 2.4631, DIN 17752, BS HR 504
  • Forms: round / hex / square bar, open-die forgings, rolled rings, discs, blanks and wire — cut or machined to drawing
  • Certification: EN 10204 3.1 mill certificate standard; 3.2 and witnessed testing arranged on request

Heat treatment, welding and purchasing notes

Heat treatment. The standard cycle is solution treatment around 1,080 °C (typically 8 h) followed by air cooling, then ageing at 700–730 °C for 16 h with air cooling. The ageing step is what develops the γ′ strength; an un-aged or under-aged part will measure soft. For extended service above 750 °C a double-age cycle can be applied — specify it at enquiry stage.

Welding. 80A is weldable but not casually: weld it in the solution-treated condition, never after ageing, because the hardened HAZ is prone to strain-age cracking. Matching-composition filler is crack-sensitive, so most fabricators join 80A to itself or to dissimilar grades with ERNiCr-3 (AWS A5.14) / ENiCr-3 (AWS A5.11) filler and age the whole assembly after welding where the specification allows. Critical rotating or pressure-boundary welds deserve a written welding procedure, not a shop-floor decision.

Purchasing. State the delivery condition explicitly — solution treated for subsequent machining, or solution treated + aged for ready-to-use fasteners — plus the governing standard (B637, AMS 5666/5702, DIN 17752), required melt route (ESR or VIM + ESR for aerospace and rotating parts) and any grain-size or ultrasonic requirements. Machine rough shapes in the solution-treated condition and age after final rough machining to avoid distortion and tooling pain; the alloy work-hardens quickly and machines best with rigid setups and sharp carbide tooling.

Frequently asked questions

Is Nimonic 80A magnetic?

No — it is essentially non-magnetic in all conditions, including the fully aged state. Any strong magnetic response usually indicates a substituted or mislabelled grade.

What is the difference between Nimonic 80A and Inconel X-750?

Both are γ′-hardened Ni-Cr superalloys. X-750 adds niobium and follows the US/AMS specification route, while 80A relies on Ti+Al alone and follows the British/European (BS HR, DIN) route. For 650–815 °C fasteners and valves they are broadly interchangeable in performance; the deciding factor is usually which specification your customer's drawing cites.

Can Nimonic 80A be welded?

Yes, with discipline: weld only in the solution-treated condition, use ERNiCr-3 / ENiCr-3 filler rather than matching wire, keep heat input low, and age after welding where the design allows. Welding an aged part invites strain-age cracking in the HAZ.

Nimonic 80A or A286 — which should I buy?

A286 is cheaper, far easier to machine and weld, and is sufficient to about 650 °C. Once continuous service pushes past ~650 °C or preload retention at temperature is critical, 80A's γ′ creep strength becomes worth the premium and the tougher machining.

What is the maximum service temperature?

About 815 °C for creep-limited duty (bolting, valves, blading). The alloy oxidises acceptably a little higher, but creep rupture strength falls rapidly above 815 °C — use Nimonic 90 for that regime.

Need Nimonic 80A (UNS N07080)?

Send us your drawing or specification for a quotation — we reply within one business day.