Haynes 230 (UNS N06230): composition, properties and applications

Haynes 230 is what you buy when the problem is not corrosion but 1,000 °C plus a thousand thermal cycles. Fourteen percent tungsten and two percent molybdenum in solid solution, a small lanthanum addition for oxide adherence, and a carbon level high enough to keep carbides at the grain boundaries: the result is an alloy that holds 98 MPa of 10,000-hour rupture strength at 760 °C, resists nitriding better than any other commercial wrought grade, and after 16,000 hours between 649 and 871 °C still shows no sigma or mu phase. This guide gives the numbers, the physical constants, and the comparison against Hastelloy X and Inconel 617 that decides most real specifications.

What Haynes 230 is — in one paragraph

Haynes 230 (UNS N06230, W.Nr 2.4733, NiCr22W14Mo) is a solid-solution-strengthened nickel-chromium-tungsten-molybdenum alloy: about 22 % Cr, 14 % W, 2 % Mo, 0.3 % Al, 0.02 % La, 0.10 % C, balance nickel. There is no gamma-prime and no ageing treatment. The tungsten is doing the heavy lifting — it is a large, slow-diffusing atom, so it raises creep resistance without the phase instability that comes with cobalt or with high aluminium-plus-titanium. Lanthanum, at 0.02 %, is there for a single purpose: it improves the adhesion of the chromia scale, which is what separates 230 from simpler Ni-Cr grades under thermal cycling.

Its reputation rests on three claims that are easy to verify. Continuous service in air up to 1,150 °C. The best nitriding resistance of any commercial wrought nickel alloy — which is why ammonia-burner catalyst grids and nitriding-furnace internals are its home ground. And long-term structural stability: after 16,000 hours at 649–871 °C, metallography shows carbides only, with no sigma or mu phase, and impact toughness stays at a usable 28–41 J. If your part is thick, hot, cycled and expected to last a decade, 230 is on the shortlist.

Chemical composition (ASTM B435 / AMS 5878)

ElementContent (wt %)Why it matters
Nickel (Ni)Balance (≈ 47–57)Austenitic matrix; the quoted minimum varies by source because Ni is reported as remainder
Chromium (Cr)20.0–24.0Oxidation resistance to 1,150 °C; chromia former
Tungsten (W)13.0–15.0The primary solid-solution strengthener. Slow-diffusing, so it holds creep strength without precipitating TCP phases
Molybdenum (Mo)1.0–3.0Secondary solid-solution strengthener; assists creep resistance
Cobalt (Co)5.0 maxDeliberately capped — this is what keeps 230 free of the cobalt price exposure that affects 617
Carbon (C)0.05–0.15Forms M6C / M23C6 carbides at grain boundaries; the creep strength depends on them
Aluminium (Al)0.20–0.50Improves scale adhesion and internal oxidation behaviour; far below the gamma-prime forming level
Lanthanum (La)0.005–0.05Rare-earth addition — the single biggest factor in cyclic oxidation life
Iron (Fe)3.0 maxResidual
Silicon (Si)0.25–0.75Oxidation resistance and casting fluidity; a range, not a maximum
Manganese (Mn)0.30–1.00Deoxidation and sulphur control
Titanium (Ti)0.10 maxKept very low on purpose — no gamma-prime, no ageing
Boron (B)0.015 maxGrain-boundary cohesion
Copper (Cu)0.50 maxResidual
Phosphorus / Sulphur0.03 max / 0.015 maxTramp elements; low S is critical for weld ductility

Two practical notes. First, the tungsten range is 13–15 % — a 2-point window on a dense, expensive element, so W content is worth checking on the certificate rather than assuming. Second, DIN 2.4733 (NiCr22W14Mo) and the ASTM composition are effectively the same alloy, but the nickel reporting convention differs between mill certificates; do not treat an apparent Ni difference as a grade problem.

Mechanical properties from room temperature to 1,150 °C

All product forms are supplied solution heat treated (nominally 1,232 °C / 2,250 °F, rapid cool). Minimum values:

Product / specification0.2 % yield (MPa)Tensile (MPa)ElongationHardness
ASTM B435 sheet, plate, strip — annealed minimum≥ 310≥ 760≥ 40 %—
AMS 5878 sheet — typical34579340 %—
AMS 5891 extruded bar — typical31075835 %≤ 241 HB
Plate, solution annealed — typical39586050 %—

The interesting curve is the hot one, and it is unusually flat. Typical tensile properties, solution-annealed plate:

Temperature0.2 % yield (MPa)Tensile (MPa)Elongation
20 °C39586050 %
540 °C27570553 %
650 °C27567555 %
760 °C27560553 %
870 °C25543565 %
980 °C14524083 %
1,095 °C7614083 %
1,150 °C4791106 %

Between 540 and 760 °C the yield strength is essentially constant at 275 MPa. That plateau is the alloy's signature: it is what lets a combustor liner or a furnace muffle keep its shape through a temperature swing that would permanently distort 601 or 800H. Elongation climbs as temperature rises, so 230 does not become brittle at 1,000 °C — it becomes soft, which is a much easier problem to design around.

Creep-rupture, stress to cause rupture in MPa:

Temperature100 h1,000 h10,000 h
650 °C385295200
760 °C18514098
870 °C956643
980 °C412111
1,040 °C2412—
1,095 °C147—
1,150 °C84—

Source: Haynes International typical rupture data for plate. These are typical values for selection work, not code allowables — ASME Code Case 2063-3 gives the design stresses for Section I and Section VIII Div. 1 construction up to 900 °C.

Physical properties

PropertyValueNotes
Density8.97 g/cm³Haynes figure; some distributor data sheets quote 9.05 g/cm³ — use the mill certificate for weight-based pricing
Melting range1,300–1,374 °CEquivalently 2,375–2,500 °F; a few sources quote 1,290–1,375 °C
Thermal conductivity8.9 W/m·K at 20 °C; 16.4 at 400 °C; 24.4 at 800 °C; 28.4 at 1,000 °CLow at room temperature — a thermal-gradient alloy, not a heat-spreader
Specific heat397 J/kg·K at 20 °C; 465 at 400 °C; 595 at 800 °C; 617 at 1,000 °C
Mean expansion coefficient12.7 ×10⁻⁶ /K (25–100 °C); 13.7 (25–400); 14.8 (25–700); 16.1 (25–1,000)Some European data sheets quote 11.8 at 100 °C; the 12.7 figure matches Haynes' own 7.0 µin/in·°F
Young's modulus211 GPa at 20 °C; 186 at 400 °C; 164 at 800 °C; 150 at 1,000 °CFalls ~29 % by 1,000 °C
Poisson's ratio0.31 (rising to ~0.34–0.35 above 600 °C in some datasets)Use temperature-specific values for hot stress analysis
Electrical resistivity1.25 µΩ·m at 20 °C≈ 125 µΩ·cm; peaks near 600 °C, then falls back
Magnetic behaviourNon-magneticAustenitic; permeability ≈ 1.00x

The low thermal conductivity is not a defect to be worked around — it is why 230 survives thermal shock. Heat moves slowly through the section, so the through-wall gradient is gentler than in a high-conductivity alloy, and the resulting thermal strain is smaller. Combine that with a moderate expansion coefficient and you get the thermal-fatigue behaviour that combustor and recuperator designers are actually buying.

Oxidation, nitriding and long-term stability

  • Oxidation: excellent in air to 1,150 °C for continuous service, which is the highest of any wrought nickel alloy in normal commercial supply. The lanthanum addition is what keeps the scale attached through cooling cycles; without it, chromia spalls and the alloy consumes itself from the outside in.
  • Nitriding: the standout property. 230 is the best commercial wrought alloy for nitrogen-bearing atmospheres, which is why it appears in nitriding-furnace fixtures, ammonia-burner catalyst grids and nitrogen-based heat-treat equipment. This is precisely where Inconel 617 is weak.
  • Carburisation: rated equal to Hastelloy X — good, not absolute. In heavy carburising atmospheres, carbon still enters and carbides still form; 230 buys you time, not immunity.
  • Sulphidation: rated equal to Hastelloy X, which is to say moderate. For high-sulphur fuel ash and reducing sulphur gases, cobalt-base alloys (Haynes 188, L-605) remain the better answer.
  • Chlorination: rated equal to 625 — usable, but this is not a wet-chlorine alloy. Aqueous chloride service belongs to C-276, C-22 or a reactive metal.
  • Structural stability: after 16,000 hours between 649 and 871 °C, no sigma, mu or other TCP phase is found — only carbides. Charpy V-notch impact falls from about 73 J in the solution-annealed condition to ~41 J after 8,000 h at 650 °C and ~28 J after 8,000 h at 760–870 °C, then plateaus. That is a predictable, designable loss of toughness, not the cliff-edge embrittlement seen in some high-chromium alloys.

Selection rule. Nitriding atmosphere, ammonia, or 1,000–1,150 °C: Haynes 230. Sustained load at 700–950 °C in an oxidising gas, or a nuclear code case: Inconel 617. Cheap 1,100–1,200 °C oxidation resistance with low load: Hastelloy X — but budget for thickness, because at 760 °C a Hastelloy X part needs roughly four times the wall of a 230 part for the same 1,000-hour rupture life (Haynes' own comparison puts 230 at about 25 % of the X thickness). Below 1,000 °C with modest stress: 601 or 253MA will usually be cheaper.

The thickness comparison is worth restating in another way, because it is the most commercially useful number in this article. Haynes publishes, for equal 1,000-hour rupture life, the thickness required relative to 230: Hastelloy X 25 %, 800H 47 %, 601 54 %, 253MA 54 %, 310 66 %, 600 71 %, 446 90 % (at 760 °C). Invert those figures and 230 carries roughly 1.9× the stress of 800H and about 1.4× that of 601 at the same wall thickness. On a high-temperature part, that difference usually pays for the alloy several times over — and it is the argument to put in front of a customer who is comparing price per kilogram.

Typical applications by industry

IndustryTypical 230 componentsWhy 230
Gas turbines / aerospaceCombustor cans, transition ducts, flame holders, liners, thermocouple sheathsOxidation to 1,150 °C plus thermal-fatigue resistance and weldability in thin sheet
Industrial furnacesRetorts, muffles, radiant tubes, belts, chains, trays, baskets, grates, rollers, fansLong-life oxidation resistance and dimensional stability at 1,000–1,150 °C
Nitriding / heat treatingNitriding-furnace internals, fixtures, jigs, sparger tubesBest-in-class nitriding resistance of any wrought nickel alloy
Chemical / fertiliserAmmonia-burner catalyst grid supports, nitric acid catalyst grids, reformer hardwareNitriding plus oxidation resistance under continuous load
Power / energyHigh-temperature heat exchangers, recuperator internals, dampers, ducting, expansion bellowsCreep strength with low thermal conductivity — smaller gradients, less distortion
EnvironmentalThermal oxidiser internals, incinerator hardware, flue-gas high-temperature sectionsOxidation and carburisation resistance in dirty combustion gas
Heat-treat equipmentBellows, furnace muffs, sensor protection tubes, strand annealing tubesCombination of formability, weldability and 1,100 °C capability

Standards and product forms

  • Sheet, plate, strip: ASTM B435 / ASME SB435; AMS 5878 (aerospace). DIN 17750
  • Bar and rod: ASTM B572 / ASME SB572; AMS 5891 (bar and forging stock)
  • Forgings: ASTM B564 / ASME SB564
  • Welded pipe: ASTM B619 / ASME SB619; seamless tube and pipe: ASTM B622 / ASME SB622; welded tube: ASTM B626 / ASME SB626
  • Fittings: ASTM B366
  • Weld consumables: ERNiCrWMo-1 (AWS A5.14) matching wire — sold by Haynes as 230-W filler
  • Design codes: ASME Code Case 2063-3 for Section I and Section VIII Div. 1, both up to 900 °C (1,650 °F)
  • Other designations: W.Nr 2.4733, NiCr22W14Mo, DIN 17744

We supply 230 as cold-rolled sheet from 0.5 mm, hot-rolled plate to 50 mm, round and peeled bar, seamless tube, and forged rings or blocks to drawing, together with ERNiCrWMo-1 filler. EN 10204 3.1 certification and PMI on every heat.

Fabrication, welding and buying notes

Heat treatment. Final solution heat treatment at 1,232 °C (2,250 °F), rapid cool, is what produces the published properties. Haynes notes that solution treatment can be run as low as about 1,163 °C, but the resulting structure and properties change — so if a drawing specifies AMS 5878 or B435 properties, do not let a fabricator substitute a lower-temperature anneal. Any hot forming or welding on a finished part should be followed by a full re-solution treatment if the part is creep-critical.

Hot forming. Work in the 1,040–1,230 °C window, with the part charged into a hot furnace, and finish above roughly 950 °C. The working range is narrow and the forces are high; a temperature drop mid-operation leads to surface cracking.

Cold forming. Readily cold formed in the annealed condition, with inter-stage anneals — the work-hardening rate is high but the ductility in the annealed state is generous (40 % elongation minimum), which is why thin combustor and bellows sections are practical in 230.

Welding. GTAW, GMAW, plasma and resistance welding all work with ERNiCrWMo-1 matching filler. No preheat and no post-weld heat treatment for most service; where the joint sees high restraint or cyclic loading, a post-weld solution anneal restores the creep properties of the HAZ. Purge the root, keep interpass below 150 °C, and remember that the low thermal conductivity means heat concentrates at the weld — a heat-input schedule that works on 310 stainless will overheat 230.

Machining. Same family behaviour as 617: work-hardening austenitic alloy, carbide tooling, rigid setup, low speed with positive feed, flood coolant, and never let the tool rub.

Buying checklist.

  • Tungsten is the identifier. XRF or lab PMI showing W at 13–15 % separates 230 from Hastelloy X (W 0.2–1.0 %), 617 (no W) and 625 (no W). This is a fast, reliable incoming check.
  • Density differs from X by nearly 9 % (8.97 vs 8.22 g/cm³). If you buy by weight and the part is thin, a heat substituted with X will be visibly lighter — weigh-check large lots.
  • Specify the product standard, not just the trade name: B435 for industrial plate and sheet, AMS 5878 for aerospace sheet, B572 for bar, B564 for forgings.
  • For code work above 900 °C, confirm that your jurisdiction accepts the code case; the ASME coverage for 230 stops at 900 °C even though the alloy runs to 1,150 °C in non-code applications.
  • Thin gauge and wide plate are the supply constraints, not the alloy itself — check mill availability before quoting a short delivery.
  • Price tracks nickel and tungsten, not cobalt. That is a structural advantage over 617 in a cobalt spike, and worth mentioning when a customer is choosing between the two.

Frequently asked questions

Is Haynes 230 age hardenable?

No. It is a solid-solution alloy strengthened by tungsten and molybdenum, supplied solution heat treated at about 1,232 °C. There is no ageing treatment, and titanium is deliberately capped at 0.10 % to prevent gamma-prime formation.

Haynes 230 versus Hastelloy X — which one?

Both resist oxidation to roughly 1,150–1,200 °C, but 230 is substantially stronger in creep: at 760 °C a Hastelloy X part needs about four times the wall thickness for the same 1,000-hour rupture life. X remains a reasonable choice for low-stress furnace hardware on a tight budget; for load-bearing parts, 230 usually wins on total cost.

Haynes 230 versus Inconel 617?

Creep strength is broadly comparable between 650 and 900 °C. Choose 230 for nitriding atmospheres, service above 1,000 °C, and thermal cycling; choose 617 for nuclear code cases and where 617 is already qualified. 230 also avoids cobalt price exposure, since Co is capped at 5 %.

What is the maximum service temperature?

About 1,150 °C continuous in clean oxidising atmospheres, which is the practical ceiling for wrought nickel alloys. ASME code coverage stops at 900 °C (Code Case 2063-3), so above that you are outside pressure-vessel rules and into engineered-component territory.

What filler metal is used for 230?

ERNiCrWMo-1 matching wire (Haynes 230-W). No preheat and normally no post-weld heat treatment; a post-weld solution anneal at about 1,232 °C is used where the joint is creep-critical or highly restrained.

Is 230 magnetic?

No. It is fully austenitic and non-magnetic in the solution-annealed condition.

Need Haynes 230 (UNS N06230)?

Send us your drawing or specification for a quotation — we reply within one business day.

Request a quote