Hastelloy X (UNS N06002): composition, properties and applications

Hastelloy X (UNS N06002, W.Nr 2.4665) is the solid-solution nickel-chromium-iron-molybdenum alloy that has defined gas-turbine combustion hardware for six decades: a Cr₂O₃-forming alloy with outstanding oxidation resistance to about 1,200 °C, good strength retention to 870–980 °C, and enough hot ductility to deep-draw the thinnest combustor liner sheet. It is emphatically not a wet-corrosion alloy — in liquid acids the C and B families do that work. This guide collects the ASTM numbers and the selection rules we use when quoting X sheet, plate, bar, tube and furnace hardware.

What Hastelloy X is — in one paragraph

Hastelloy X (UNS N06002) is a solid-solution nickel-base alloy with roughly 21–23 % chromium, 18 % iron, 9 % molybdenum, 0.5–2.5 % cobalt and 0.2–1 % tungsten. The chromium forms a slow-growing, tenacious Cr₂O₃ scale that resists oxidation and spalling through extreme thermal cycling, while Mo + W carry the solid-solution strength. With 47 %+ nickel, X is immune to chloride stress-corrosion cracking, resists carburisation better than stainless steels, and — unusually for a 1,200 °C-class alloy — stays highly formable and weldable without ageing treatments. It has been the standard sheet alloy for combustor cans and transition ducts since the 1960s and remains the reference for industrial-furnace hardware in mixed atmospheres.

Chemical composition (ASTM B435 / B572, UNS N06002)

ElementContent (wt %)Why it matters
Nickel (Ni)Balance (≈ 45–52)Austenitic base; chloride-SCC immunity and hot-strength foundation
Chromium (Cr)20.5–23.0Cr₂O₃ protective scale — oxidation resistance to ~1,200 °C and spalling resistance under thermal cycling
Iron (Fe)17.0–20.0Cost and processability; keeps the structure fully austenitic
Molybdenum (Mo)8.0–10.0Solid-solution strengthening; retains yield at elevated temperature
Cobalt (Co)0.5–2.5Hot-strength and microstructure stability
Tungsten (W)0.2–1.0Secondary solid-solution strengthener
Carbon (C)0.05–0.15Deliberately NOT low — carbides pinned on grain boundaries give creep/rupture strength above ~800 °C (see FAQ)
Manganese / Silicon1.0 max eachDeoxidation and processing control

Mechanical properties

Minimum values in the solution-annealed condition, with typical mill values in brackets:

Condition / productYield strength (0.2 %)Tensile strengthElongation
ASTM B435 sheet / B572 bar — annealed minimum≥ 240 MPa≥ 655 MPa (95 ksi)≥ 35 %
Typical mill sheet (RT, annealed)[360–380][760–790][43–49]
Typical mill plate (RT, annealed)[≈ 340][≈ 760][≈ 49]

Where X actually earns its keep is the elevated-temperature table — published typical tensile data for annealed sheet:

TemperatureTensile strengthYield strength (0.2 %)Elongation
538 °C (1,000 °F)≈ 628 MPa≈ 253 MPa≈ 54 %
649 °C (1,200 °F)≈ 580 MPa≈ 241 MPa≈ 66 %
760 °C (1,400 °F)≈ 424 MPa (≈ 54 % of RT tensile)≈ 233 MPa≈ 96 %
871 °C (1,600 °F)≈ 251 MPa≈ 193 MPa≈ 118 %

Note that some producer tube specifications (e.g. AMS 5588 stockists) quote 827 MPa UTS / 345 MPa YS minimums for annealed tube — stricter than the generic B435/B572 table. Always compare like with like: product spec, product form, condition.

Physical properties

PropertyValue
Density8.22 g/cm³
Melting range1,260–1,355 °C
Thermal conductivity (≈ 25 °C)≈ 9.2 W/m·K
Specific heat (RT)≈ 486 J/kg·K
Thermal expansion (26–100 °C)≈ 13.9 ×10⁻⁶ /K
Electrical resistivity (≈ 24 °C)≈ 1.15 µΩ·m
Modulus of elasticity (RT)≈ 205–207 GPa
Magnetic behaviourEssentially non-magnetic (µ ≈ 1.002)
Recommended solution anneal≈ 1,177 °C (2,150 °F), rapid cool

High-temperature performance — and the wet-corrosion caveat

  • Oxidation: exceptional resistance to about 1,200 °C in air or oxidising flue gas; the Cr₂O₃ scale survives severe thermal cycling with minimal spalling. This is the property that made X the combustor-liner standard.
  • Mixed atmospheres: performs in oxidising, neutral and intermittently reducing furnace atmospheres — furnace rolls, trays and mesh made of X run for thousands of hours without scaling or distortion.
  • Carburisation: clearly better carburisation resistance than standard stainless steels, a key reason it appears in ammonia and ethylene cracker hardware (catalyst support grids, furnace pigtails).
  • Hot strength: still ~54 % of its room-temperature tensile strength at 760 °C and useful stress-rupture properties well past 870 °C.
  • The caveat: X was optimized for hot, dry duty. In liquid acids — hot concentrated HCl, H₂SO₄, wet process streams — the C-family (C-276, C-22) and B-family (B-2, B-3) are the correct Hastelloys; X will disappoint there.

Selection rule of thumb: if the duty is hot gas — combustion, furnace, exhaust, carburising — X is the first alloy to price. If the duty is liquid acid, move straight to C-276 / C-22 / B-3 and do not pay X prices for a wet-corrosion job it was never designed for.

Typical applications

IndustryTypical Hastelloy X components
Aerospace / gas turbinesCombustor cans and liners, transition ducts, afterburner components, tailpipes, spray bars
Industrial furnaces / heat treatmentFurnace rolls, retorts, trays, baskets, radiant tubes, support mesh and fixtures
PetrochemicalCatalyst support grids and furnace components in ammonia and ethylene production; reformer and cracker internals
Power / nuclearHigh-temperature heat-exchanger and reactor-system components, gas-cooled reactor hardware
Commercial heat processing Brazing and annealing fixtures, muffles, thermocouple protection tubes in mixed atmospheres

Standards and product forms we supply

  • Plate / sheet / strip: ASTM B435 / ASME SB435; AMS 5536 (aviation sheet)
  • Bar / rod / forgings: ASTM B572 / ASME SB572; AMS 5754
  • Seamless pipe & tube: ASTM B622 / ASME SB622; AMS 5588 (tubes)
  • Welded pipe & tube: ASTM B619 / B626 / ASME SB619 / SB626
  • Weld wire / electrodes: ERNiCrMo-2 (AWS A5.14), ENiCrMo-2 (AWS A5.11)
  • European equivalent: W.Nr 2.4665 / NiCr22Fe18Mo
  • Forged rings, flanges and machined parts: supplied to drawing with EN 10204 3.1 certificates

Fabrication, welding and buying notes

  • Welding: straightforward for a superalloy — GTAW/GMAW with ERNiCrMo-2 filler, no preheat, no post-weld heat treatment required for furnace and combustor service. X is notably resistant to strain-age cracking, which is one reason it displaced harder-to-weld alloys in repair work.
  • Forming: in the annealed state X deep-draws and spins well — combustor cans are literally deep-drawn from thin sheet. For heavy cold work, a solution anneal restores full ductility before further forming.
  • Condition discipline: order "solution annealed" (≈1,177 °C, rapid cool) for forming and welding; the as-delivered condition matters more here than on corrosion grades because hot strength and ductility both depend on it.
  • Buying: for aerospace-adjacent work, specify the AMS document (5536 sheet / 5754 bar / 5588 tube) alongside ASTM — the AMS table is what the aviation QA system audits. For furnace hardware, ASTM B435/B572 plus EN 10204 3.1 is normally sufficient.

Frequently asked questions

Is Hastelloy X magnetic?

No — annealed X is essentially non-magnetic (permeability ≈1.002). It is a fully austenitic solid-solution alloy with no age-hardening phases.

Can Hastelloy X be age hardened?

No. X is a solid-solution alloy; its high-temperature strength comes from Mo/W in solution plus grain-boundary carbides, not from ageing precipitates. If your specification asks for age-hardening heat treatments, you are probably thinking of Inconel X-750, Waspaloy or Nimonic grades.

Why is the carbon range 0.05–0.15 % — shouldn't it be low-carbon like 316L?

No. The deliberately wider carbon range sustains grain-boundary carbide precipitation, which pins the boundaries and provides creep-rupture strength above about 800 °C. Sensitisation rules from stainless steel do not apply here — X spends its life at temperatures where those carbides are an asset, not a liability.

Hastelloy X vs C-276 — they are both 'Hastelloy', what's the difference?

Different jobs. X is a high-temperature alloy (oxidation to ~1,200 °C, combustion and furnace duty); C-276 is a wet-corrosion alloy (hot HCl, H₂SO₄, mixed acids). Choosing X for liquid-acid service — or C-276 for a 1,000 °C furnace roll — are the two most common specification errors with this family.

What is the maximum service temperature?

Oxidation resistance extends to about 1,200 °C, but structural usefulness depends on stress: components carrying meaningful load are typically designed in the 870–980 °C band, where X still retains significant strength. For load-bearing furnace parts above that, Waspaloy or cobalt alloys such as Haynes 188 / 230-class alloys enter the conversation.

Need Hastelloy X (UNS N06002)?

Send us your drawing or specification for a quotation — we reply within one business day.