Ferralium 255 (UNS S32550 / 1.4507): the copper-bearing super duplex for acid and pump duty

Ferralium 255 is the duplex grade that was designed around a different question. Where 2205 and 2507 chase higher and higher pitting resistance, 255 keeps 25 % chromium and 3.5 % molybdenum but adds 1.5-2.5 % copper on purpose, buying resistance to dilute sulphuric and phosphoric acid that the standard duplex grades simply do not have. This guide collects the ASTM minima, the physical data, the PREN arithmetic that decides whether a heat qualifies as super duplex at all, and the purchasing checks we run before shipping S32550 plate, bar, forgings and pump components.

Duplex stainless flanges at an oil and gas yard

What Ferralium 255 is — in one paragraph

Ferralium 255 (UNS S32550, W.Nr 1.4507, X2CrNiMoCuN25-6-3, ASTM A182 grade F61) is a 25 % chromium duplex stainless steel with roughly 45-55 % ferrite and 45-55 % austenite, strengthened by nitrogen and modified by an intentional copper addition of 1.5-2.5 %. It was patented by Langley Alloys in 1968 and is generally credited as the first nitrogen-bearing super duplex, which is why the trade name is still more widely recognised than the UNS number.

The copper is the whole point. In a chloride environment 255 behaves like a mid-range super duplex; in a dilute reducing acid — sulphuric, phosphoric, many organic acids — it behaves noticeably better than 2205 or 2507, because copper raises the potential at which the passive film breaks down in those specific media. That combination of 550 MPa yield, PREN 38-41 and acid resistance is why the grade survives commercially in slurry pumps, valve trim, phosphoric acid plants and hydrometallurgy, where a 904L impeller would be too weak and a 2507 impeller would corrode.

Think of the family as a ladder rather than a ranking: 2205 (PREN ≈ 35, 450 MPa yield, no copper) → Ferralium 255 (PREN 38-41, 550 MPa, 1.5-2.5 % Cu) → 2507 (PREN 41-43, 550 MPa, higher nitrogen) → Zeron 100 (PREN ≈ 40-42, tungsten plus copper). Each step buys one specific property and pays for it in price, availability and welding discipline.

Nominal chemical composition

Heat analysis per ASTM A240 for UNS S32550 (wt %):

ElementContent (wt %)What it does in 255
Chromium (Cr)24.0-27.0Passive film former; sets the base pitting resistance and the oxidation limit
Nickel (Ni)4.5-6.5Balances the austenite/ferrite ratio at roughly 50/50; low Ni is deliberate — it is what keeps the alloy duplex rather than austenitic
Molybdenum (Mo)2.9-3.9Pitting and crevice resistance, plus general corrosion resistance in reducing media
Copper (Cu)1.50-2.50The design intent: raises resistance in dilute sulphuric and phosphoric acid and improves erosion-corrosion behaviour in slurries
Nitrogen (N)0.10-0.25Solid-solution strengthening (most of the 550 MPa yield) and fast austenite reformation in the weld HAZ
Carbon (C)0.04 maxKept low to limit carbide precipitation; note this is looser than the 0.030 max of 2205/2507
Manganese (Mn)1.50 max Austenite former and deoxidation; high Mn is not wanted in seawater duty
Silicon (Si)1.00 maxDeoxidation; excessive Si promotes intermetallic phases
Phosphorus / Sulphur (P / S)0.040 / 0.030 maxResiduals. The 0.030 % S ceiling is generous — offshore specifications usually tighten it to 0.010 %
Iron (Fe)BalanceMatrix

Two certification traps are worth knowing before you release a heat.

First, EN 1.4507 is not the same window as A240. EN 10088-3 describes 1.4507 as Cr 24-26, Ni 6-8, Mo 3-4, N 0.20-0.30, Cu 1-2.5, C 0.03 max. A240 allows Ni 4.5-6.5 and N 0.10-0.25. A heat can only carry both certificates if it lands in the overlap — Ni 6.0-6.5 and N 0.20-0.25 — which means a "dual certified" plate is a narrower, more expensive heat than either single specification requires. If a supplier offers dual certification at the price of a plain A240 plate, ask for the heat analysis rather than the grade line on the certificate.

Second, the low-sulphur requirement is not cosmetic. Sulphur improves machinability but manganese sulphide inclusions are preferred pitting sites. For pump and seawater duty we default to S ≤ 0.010 % even though A240 permits 0.030 %.

Mechanical properties by product form

Minimum values required by the ASTM product specifications, with typical mill-certificate ranges in brackets:

Product form0.2 % yieldTensile strengthElongation (50 mm)Hardness
Plate / sheet / strip — ASTM A240, annealed≥ 550 MPa≥ 760 MPa≥ 15 %≤ 302 HBW or ≤ 32 HRC
Bar / rod — ASTM A276≥ 550 MPa≥ 760 MPa≥ 15 %≤ 302 HBW
Forgings / flanges — ASTM A182 F61≥ 550 MPa≥ 760 MPa≥ 15 %≤ 302 HBW
Tube — ASTM A789 / A790≥ 550 MPa≥ 760 MPa≥ 15 %≤ 302 HBW
Typical mill values, solution annealed586-650 MPa790-880 MPa25-28 %≤ 270 HBW
255-SD50 (producer grade, section ≤ 300 mm)≥ 586 MPa guaranteed≥ 800 MPa≥ 25 %—

Watch the datasheets: 485 MPa / 690 MPa / 25 % is often quoted for "255" and it is not the ASTM A240 requirement. Those figures come from cast or proprietary product data. If your purchase order says ASTM A240 UNS S32550, the enforceable numbers are 550 / 760 / 15 % and 302 HBW — put them on the order and reject anything below.

Notes that matter in design:

  • Elongation of 15 % is a floor, not a target. A well-annealed heat runs 25-28 %. A plate that only reaches 17-18 % is usually evidence of a slow quench and some sigma phase, not of a "tight" heat.
  • Hardness is the cheapest quality gate you have. Duplex that has been slowly cooled from the annealing temperature hardens; anything above 270 HBW deserves an ASTM A923 or G48 check before it goes into a pump.
  • Impact toughness is not an A240 requirement. For low-temperature or offshore duty, specify 45 J average at −46 °C (typical mill results are around 80 J) — this is where a bad heat becomes visible.
  • Section size does cost strength. The guaranteed 586 MPa of the SD50 producer grade applies to sections up to 300 mm; beyond that, discuss the actual forging reduction ratio with the mill.

Physical properties

Typical values from producer data compiled in the IMOA duplex guide; they are reference values, not ASTM requirements.

PropertyValue
Density7.82 g/cm³ (some sources 7.80)
Melting range≈ 1,400-1,450 °C (some sources 1,390-1,440 °C)
Thermal conductivity, 20 °C14.3 W/m·K
Thermal conductivity, 100 °C / 200 °C / 300 °C16.4 / 18.6 / 19.1 W/m·K
Specific heat capacity488 J/kg·K
Thermal expansion, 20-100 °C12.1 ×10⁻⁶ /K
Thermal expansion, 20-200 °C / 20-300 °C / 20-400 °C12.6 / 13.0 / 13.3 ×10⁻⁶ /K
Young's modulus, 20 °C210 GPa
Young's modulus, 100 °C / 300 °C / 500 °C200 / 192 / 170 GPa
Electrical resistivity0.84 µΩ·m
Magnetic behaviourFerromagnetic — both phases are magnetic, unlike 316L or 904L
Ferrite content≈ 45-55 % (NACE requires 35-65 %)

Three practical consequences. The thermal expansion is about 30 % higher than carbon steel, so dissimilar-metal welds and long pipe runs need the expansion loops you would give a 304 line, not a carbon steel one. The thermal conductivity is roughly half that of carbon steel, which makes 255 prone to local overheating under a torch or a poor grinding pass. And the magnetic response is normal: a magnet test tells you nothing about whether the heat is correct, and a fabricator who "demagnetises" the plate is solving a problem that does not exist.

Corrosion resistance — where the copper earns its price

PREN for 255 is calculated as Cr + 3.3 Mo + 16 N (no tungsten in this grade):

  • Specification minimum — 24.0 Cr, 2.9 Mo, 0.10 N: PREN ≈ 35.2
  • Typical heat — 25.5 Cr, 3.4 Mo, 0.175 N: PREN ≈ 39.5
  • Published range — IMOA quotes 38-41; some producers and distributors quote up to 43

The ASTM A240 composition window, taken at its minima, computes to a PREN of 35.2 — the same pitting resistance as 2205, not a super duplex at all. If your project specification, NORSOK M-630 clause or end-user datasheet calls for "super duplex", the purchase order must state "PREN ≥ 40, calculated from the heat analysis and reported on the mill certificate". Without that sentence you can legally receive a heat that is 5 points below the grade's reputation.

What the copper actually does:

  • Dilute sulphuric acid. This is the historical justification for 255. In low-concentration, low-aeration sulphuric acid streams the copper raises the corrosion potential and suppresses active dissolution, giving service life where 2205 and 2507 pit and general-corrode. The benefit is largest in dilute, mildly aerated streams and disappears in concentrated acid or in strongly oxidising conditions — always check an isocorrosion chart for your actual concentration and temperature rather than extrapolating.
  • Phosphoric acid and fertiliser duty. Wet-process phosphoric acid carries chlorides, fluorides and solids. 255 is a standard choice for slurry pump casings, agitators and piping in this circuit; it is not immune, but it wears and corrodes more slowly than 2205 and is far stronger than 904L.
  • Chlorides and seawater. PREN 38-41 puts 255 between 2205 and 2507. Ambient-temperature seawater is comfortable; above roughly 40-50 °C, or where chlorination and crevices combine, 2507 or Zeron 100 is the safer specification. 255 is not a substitute for 6Mo austenitics in hot concentrated chlorides.
  • Stress-corrosion cracking. The ferrite phase blocks transgranular chloride SCC, which is why duplex grades are used for hot chloride service where 304/316 would crack. For sour service, NACE MR0175 / ISO 15156-3 permits S32550 with ferrite 35-65 % and hardness ≤ 28 HRC — both conditions must be stated on the order, because A240 itself allows 302 HBW (≈32 HRC).
  • Abrasion-corrosion. The strain-hardening behaviour of the austenite phase gives 255 slightly better cavitation and slurry erosion resistance than 2205 at the same hardness. In pump impellers this often matters more than the PREN figure.

Where not to use it: strongly oxidising acids such as nitric, hot concentrated sulphuric acid, and any stream where free halogens are present. In those media the copper addition is at best neutral and the duplex microstructure is at worst a liability.

Temperature limits and the two embrittlement windows

Duplex stainless is not a high-temperature material, and 255 is no exception. Three windows matter:

WindowWhat happensDesign consequence
−46 to +300 °CNormal service range; toughness and corrosion resistance stablePressure duty up to about 300 °C. ASME BPVC Section VIII Div. 1 lists duplex grades only to 315 °C — verify the edition and the exact grade line before designing above 300 °C
300-500 °C (fastest ≈475 °C)Spinodal decomposition of the ferrite ("475 °C embrittlement")Hardness and the ductile-brittle transition rise. A part that passed 45 J at −46 °C at delivery can fail it after a long hold in this band
600-950 °C (fastest 800-850 °C)Sigma and chi phase precipitationCatastrophic loss of toughness and corrosion resistance. This is why annealing runs at ≥1,040 °C with rapid cooling, why no post-weld heat treatment is ever specified, and why hot-formed parts need a full re-anneal

If the duty needs more than 300 °C, the answer is not "a better duplex" — it is a different family: 904L or Alloy 20 for corrosion at moderate temperature, 310S/800H for oxidation, or a nickel alloy for both. Pushing 255 past 300 °C usually ends in a failed impact test at the next shutdown inspection.

Low temperature is more forgiving: duplex retains useful toughness to about −50 °C, and impact testing at −46 °C is standard offshore practice. It is not a cryogenic material — for LNG or liquid nitrogen duty, use austenitic 304L/316L or an aluminium alloy.

Selecting between 255 and its neighbours

GradePRENYield minCuIndicative cost vs 2205Choose it when
2205 (S32205)34-36450 MPanone1.0General chloride duty, ambient seawater, cost-driven projects with no acid component
Ferralium 255 (S32550)38-41550 MPa1.5-2.5 %≈ 1.4-1.7×Dilute sulphuric or phosphoric acid plus chlorides and abrasion: pumps, valve trim, agitators, hydromet
2507 (S32750)41-43550 MPanone≈ 1.5-1.8×Maximum pitting/crevice resistance, hot seawater, heavy weld fabrication (0.27 N stabilises the HAZ better)
Zeron 100 (S32760)40-42 (W credited)550 MPa0.5-1.0 %≈ 1.8-2.2×Sour service and hot seawater where a tungsten-bearing super duplex is named
904L (N08904)34-36220 MPa1.2-2.0 %≈ 2.0-2.5×Welded acid equipment needing ductility and no 475 °C risk; strength is not the driver
Alloy 20 (N08020)26-31241 MPa3-4 %≈ 2.5-3.0×Hot sulphuric acid with chlorides; cast pump bodies and valve trim in fertiliser plants

Cost multiples are indicative and move with the nickel, molybdenum and copper surcharges — treat them as an order-of-magnitude guide for early-stage selection, not as a quotation.

The substitution trap. F61 (255) and F53 (2507) sit next to each other in ASTM A182 and are frequently swapped by traders. They are not interchangeable. Supplying F53 against an F61 order deletes the copper and therefore the acid resistance the design was based on — that requires an engineering deviation, which in fertiliser and hydromet projects is rarely granted. Supplying F61 against an F53 order may be technically tolerable for plain chloride duty, but the PREN can fall below 40 and disqualify the alloy under NORSOK M-630, so it needs buyer approval plus heat-by-heat PREN verification.

Fast field test: 255 contains 1.5-2.5 % copper and 2507 does not. A handheld XRF or OES reading that shows no copper, on a part stamped F61, is proof of substitution — and it takes thirty seconds. We run this check on every 255 shipment before packing.

Applications by industry

IndustryTypical 255 componentsWhy 255 rather than 2205 or 2507
Pulp & paper pumpsImpellers, casings, wear rings, shaft sleeves, stock pumpsAcid + chloride + abrasive stock: the copper helps in the reducing acid, the duplex structure resists cavitation
Phosphoric acid / fertiliserSlurry pumps, agitators, reactor internals, transfer piping, heat-exchanger tubesWet-process acid carries chlorides and solids; 904L is too weak, 2507 corrodes in the reducing acid
Dilute sulphuric acid & hydrometallurgyMixer-settler internals, SX-EW pumps, laterite leach slurry lines, autoclave flash vesselsDocumented service history in Cu-bearing duplex; erosion-corrosion resistance in slurries
Seawater & desalinationRO high-pressure pump bodies, brine pumps, firewater pump casings, valve bodiesAmbient seawater with 550 MPa yield; step up to 2507 above ~40-50 °C or in chlorinated crevices
Flue-gas desulphurisation & miningLimestone slurry pumps, hydrocyclones, chutes, agitator shaftsAbrasion plus acidic chloride condensate — the combination that wears out 2205 quickly
Oil & gas (moderate sour)Valve bodies and trim, small forgings, flowline componentsNACE-qualified when ferrite 35-65 % and ≤28 HRC; for high H₂S partial pressure use Zeron 100 or 2507
Marine hardwareShafting sleeves, stern-gland components, fasteners above the waterlineStrength and corrosion in one piece; not for immersed high-stress shafts where 2507 is preferred

The pattern is consistent: 255 wins where a pump or valve has to survive acid, chloride and solids at the same time. Where there is no acid, 2205 is cheaper and perfectly adequate; where there is no abrasion but extreme chloride, 2507 is better.

Standards and product forms

Product formStandardNotes
Plate, sheet, stripASTM A240 / ASME SA-240Solution annealed ≥1,040 °C, rapid cooling, pickled or descaled
Bar and rodASTM A276, A479A479 for pressure-retaining bar stock in vessels
Forgings, flanges, fittings stockASTM A182 grade F61F61 is the correct marking; F53 is 2507
Seamless and welded tubeASTM A789 / A790Check that the tube specification explicitly lists S32550 — not all editions do
Pipe fittingsASTM A815 (UNS S32550)Butt-weld and forged fittings
European designationEN 10088-2 / -3, 1.4507Narrower window than A240 — see the composition section
Chinese designationGB/T 21833, 03Cr25Ni6Mo3Cu2N (S25554)Common for domestic pump castings and forgings
Japanese designationJIS SUS 329J4L—
Sour serviceNACE MR0175 / ISO 15156-3Ferrite 35-65 %, hardness ≤28 HRC, heat treated per the standard
Offshore procurementNORSOK M-630 (MDS), M-650 qualificationPREN ≥ 40 is normally written into the MDS — this is where the A240 minimum fails

Forms we supply: plate 3-60 mm, round bar 12-250 mm, forged rings, blocks, flanges and valve bodies to drawing, seamless tube, and machined pump components. Ferralium 255 is a Langley Alloys trademark: if your purchase order names the trademark rather than UNS S32550, either the mill must be Langley or you need a documented equivalence approval before shipment.

Welding and fabrication

255 welds like a super duplex, which is to say: easily, provided you respect the phase balance and the cooling rate.

  • Filler metal: ER2594 (25 9 4 N L) for general and chloride duty; ER2553 (25 9 4 Cu L) when the joint itself must retain the copper-bearing acid resistance, which is what most acid-service specifications ask for. Do not use ER2209 — the lower alloy content under-matches both strength and corrosion resistance.
  • Heat input: 0.5-2.5 kJ/mm, stringer beads, interpass temperature ≤150 °C. High heat input coarsens the ferrite and gives time for sigma and nitride precipitation.
  • No preheat, no PWHT. Post-weld heat treatment is not merely unnecessary, it is harmful — any hold in the 600-950 °C window precipitates sigma. If a specification asks for stress relief, challenge it and propose full solution annealing instead.
  • Purge: argon with 2-3 % nitrogen on the root, oxygen below 50 ppm. Nitrogen in the purge gas is what re-forms austenite in the root bead; without it the root stays ferritic and corrodes first.
  • Cleaning: pickle and passivate after welding. Iron contamination from carbon steel tooling is the single most common cause of early pitting on duplex fabrications — use dedicated stainless brushes and grinding discs.
  • Dissimilar joints: to carbon steel use ER309MoL or ER2594 with a buttered layer; nickel-base ERNiCrMo-3 is the safe choice for highly restrained joints.

Machining is where most first-time users lose money. 255 work-hardens faster than 316L, so light cuts and dwelling are the enemy: use sharp carbide, positive rake, heavy feed and constant engagement, and never let the tool rub. Drilling deep holes needs a peck cycle and generous coolant. Cold forming is possible but springback is roughly double that of austenitic stainless because of the 550 MPa yield — over-bend accordingly, and anneal between severe operations.

Purchasing checklist — the six lines that prevent a bad heat

#Requirement to write on the POWhy
1UNS S32550, ASTM A240 (or A276 / A182 F61 / A789), solution annealed ≥1,040 °C, rapid cooledLocks the grade and the heat treatment; a slow-cooled plate is the most common failure mode
2PREN ≥ 40 calculated from the heat analysis and reported on the certificateThe composition minima only compute to 35.2; without this line the "super duplex" claim is unenforceable
3Hardness ≤ 270 HBW (≤ 28 HRC if NACE MR0175 applies), tested on every pieceThe cheapest proxy for correct quench and for sour-service compliance
4Ferrite 35-65 % by point count, reported per heatRequired by NACE; also catches unbalanced heats that weld badly
5Charpy 45 J average at −46 °C (three specimens) for low-temperature or offshore dutyNot an A240 requirement — must be bought explicitly
6EN 10204 3.1 certificate, PMI with copper reported, ASTM G48 Method A on requestCopper is the discriminator against 2507; G48 catches sigma and wrong annealing

The single most useful check on a 255 delivery is also the cheapest: an XRF reading of copper. 1.5-2.5 % Cu confirms 255; 0 % Cu with a matching chromium level means you have been shipped 2507, and 0 % Cu with lower chromium means 2205. Neither will perform in the acid service the part was designed for.

Lead times are realistic at 30-45 days for plate and bar from mill stock plus processing, and 45-70 days for forged or machined pump components. Anyone quoting 255 from stock in a wide size range is usually quoting a substitute — ask for the heat number before you celebrate the delivery date.

Buying Ferralium 255 from Hangbo

We supply UNS S32550 plate, bar, forged rings, flanges and machined pump and valve components against ASTM A240 / A276 / A182 F61, with EN 10204 3.1 certificates as standard. Every lot is PMI-verified with copper reported, hardness-tested, and — where the specification calls for it — impact tested at −46 °C and checked to ASTM G48.

Typical lead time is 30-45 days for plate and bar, 45-70 days for forged and machined parts. If you are replacing a 2507 or 2205 component because of an acid-side corrosion failure, send us the medium, concentration, temperature and the failed part's condition — we will tell you whether 255 is genuinely the right step, or whether the duty actually needs Alloy 20 or a nickel alloy.

Frequently asked questions

Is Ferralium 255 the same as 2507?

No. Both are 25 % Cr duplex with about 550 MPa yield, but 255 carries 1.5-2.5 % intentional copper and a lower nitrogen range, giving PREN 38-41 against 41-43 for 2507. The copper buys dilute-acid resistance; 2507 buys chloride pitting margin and better HAZ stability when welding thick sections. The forging grades are F61 and F53 respectively and are not interchangeable on a purchase order.

Is 255 magnetic?

Yes. Both the ferrite and the austenite in a duplex steel respond to a magnet, and the ferrite content of about 50 % makes the response strong. Magnetism is not an indication of a wrong grade or of heat damage.

What is the maximum service temperature?

About 300 °C for pressure duty. Between 300 and 500 °C the ferrite embrittles (fastest near 475 °C) and between 600 and 950 °C sigma phase forms. ASME Section VIII Div. 1 lists duplex grades only up to 315 °C, so a design above 300 °C needs a code check rather than a catalogue value. For hotter corrosive duty, move to 904L, Alloy 20 or a nickel alloy.

Why does the PREN on my certificate read 36 when the datasheet says 40+?

Because ASTM A240 sets composition minima, not a PREN minimum. At 24.0 % Cr, 2.9 % Mo and 0.10 % N the formula gives 35.2. A heat inside the specification can therefore be ordinary duplex in performance. Write 'PREN ≥ 40 calculated from heat analysis' on the order and require it on the mill certificate.

Can 255 replace 904L in sulphuric acid service?

Often yes, and with more than double the yield strength — but the two are not equivalent. 904L is austenitic, welds and forms more easily and has no 475 °C embrittlement issue; 255 is stronger and cheaper per unit strength but sensitive to heat treatment discipline. Check the actual concentration and temperature against an isocorrosion chart for both grades before switching, especially above 60 °C.

Do you need to post-weld heat treat 255?

No — and you should not. Any hold in the 600-950 °C range precipitates sigma phase and destroys toughness and corrosion resistance. Correct practice is controlled heat input (0.5-2.5 kJ/mm), interpass below 150 °C, nitrogen-purged root, and pickle/passivate afterwards. If a specification demands stress relief, propose full solution annealing at ≥1,040 °C with rapid cooling instead.

How do I know I have not been shipped 2507 instead?

Read the copper. 255 contains 1.5-2.5 % Cu; 2507 contains none. A handheld XRF or a laboratory OES check takes seconds and is the definitive field test. Confirm the marking is F61 (255) and not F53 (2507) as well, and ask for the heat analysis rather than the grade line on the certificate.

Need Ferralium 255 (UNS S32550)?

Send us your drawing or specification for a quotation — we reply within one business day.