310S / 310H (UNS S31008 / S31009): the 25 % Cr – 20 % Ni heat-resistant austenitic

310S is the standard answer when a part has to sit in a furnace at 1,000–1,150 °C in air and keep its shape: 25 % chromium for a scaling-resistant oxide, 20 % nickel to hold a fully austenitic structure at temperature, and low carbon so welds do not sensitize. 310H is the same steel with carbon deliberately raised to 0.04–0.10 % for creep strength above roughly 600 °C. This guide covers both, the carbon decision between them, the sigma-phase window that catches most first-time users, and the fabrication rules that keep furnace parts from cracking in service.

Stainless steel seamless tubes in warehouse

What 310S / 310H is — in one paragraph

310S (UNS S31008, W.Nr 1.4845, JIS SUS310S, GB 06Cr25Ni20) is a high-chromium, high-nickel austenitic stainless steel — nominally 25 % Cr, 20 % Ni, carbon capped at 0.08 % — designed for service where oxidation resistance and structural stability at temperature matter more than room-temperature strength. It is the workhorse heat-resistant grade of the 300 series: it resists scaling in air to about 1,150 °C in continuous duty, stays fully austenitic (so it does not embrittle by the ductile-brittle transition that limits ferritic heat-resistant steels), and welds with ordinary stainless practice. 310H (UNS S31009) is the same composition with carbon specified at 0.04–0.10 % instead of 0.08 % max; the higher carbon raises creep and rupture strength above roughly 550–600 °C, at the cost of somewhat greater carbide precipitation. The basic 310 grade (UNS S31000) allows carbon up to 0.25 % and is essentially obsolete for new work.

Think of the family as a ladder by temperature: 309S (22 Cr / 13 Ni) to about 980 °C, 310S to about 1,050–1,100 °C continuous, 310H where creep design governs above 600 °C, and 314 (25/20 with ~2 % Si) or 253MA where cyclic scaling or higher creep strength is needed. Above roughly 1,150 °C, or in sulphur-bearing or reducing atmospheres, the answer moves to nickel-base grades — 600, 601 or 693.

Nominal composition: 310S versus 310H

Element310S (S31008)310H (S31009)Why it matters
Chromium (Cr)24.0–26.024.0–26.0Forms the Cr2O3 scale that gives oxidation resistance to ~1,150 °C
Nickel (Ni)19.0–22.019.0–22.0Stabilizes austenite, keeps high-temperature toughness, resists chloride SCC
Carbon (C)0.08 max0.04–0.10The only real difference: carbon raises creep strength and carbide volume
Silicon (Si)1.50 max1.50 maxImproves scaling resistance; higher Si (314) extends it further
Manganese (Mn)2.00 max2.00 maxAustenite former, deoxidation
Phosphorus / Sulphur0.045 / 0.030 max0.045 / 0.030 maxResiduals; sulphur affects weldability
Iron (Fe)BalanceBalanceMatrix

310S and 310H are metallurgically the same steel separated by a carbon band. A mill certificate for 310S must show C ≤ 0.08 %; for 310H, C between 0.04 and 0.10 %. Because both are 25/20, a PMI gun cannot tell them apart — the carbon value on the certificate is the only proof, so always state S31008 or S31009 on the purchase order and check the heat analysis on arrival.

Mechanical properties

Room-temperature floors are identical for the two grades; the difference appears only in elevated-temperature design allowables.

Grade / form0.2 % yieldTensile strengthElongationHardness
310S plate — ASTM A240 (annealed)≥ 205 MPa [230–290]≥ 515 MPa [550–650]≥ 40 % [45–55]≤ 95 HRB (≈ 150–180 HB typical)
310S bar — ASTM A276 (annealed)≥ 205 MPa≥ 515 MPa≥ 40 %≤ 95 HRB
310S pipe — ASTM A312 / A213 (annealed)≥ 205 MPa≥ 515 MPa≥ 35–40 %—
310H plate — ASTM A240 (annealed)≥ 205 MPa≥ 515 MPa≥ 40 %≤ 95 HRB
Cold-worked sheet / stripagreed on order700–900 MPa15–30 %—

Three practical points. First, 205 MPa yield is low by modern standards — these grades are selected for temperature capability, not for load-bearing efficiency at room temperature; if you need strength at 20 °C, use duplex or a precipitation-hardening grade. Second, 310H does not give higher room-temperature values: its benefit is entirely in the creep and rupture regime, where ASME II-D tabulates higher allowable stresses for 310H than for 310S above roughly 550–600 °C. Third, the annealed condition is soft and ductile, which is what you want for formed furnace furniture, but cold work from bending or straightening raises yield quickly and can leave residual stress that matters in cyclic service.

Physical properties

PropertyTypical value
Density7.98 g/cm³ (some sources 7.95 — within normal product tolerance)
Melting range≈ 1,400–1,450 °C
Thermal conductivity≈ 14.2 W/m·K at 100 °C; rises to ≈ 18–19 W/m·K at 500 °C
Specific heat (20 °C)≈ 500 J/kg·K
Mean expansion (20–100 °C)≈ 15.9 ×10⁻⁶ /K (≈ 16.5 ×10⁻⁶ /K average over 20–1,000 °C)
Modulus of elasticity (20 °C)≈ 200 GPa
Electrical resistivity (20 °C)≈ 0.78 µΩ·m
Magnetic behaviourNon-magnetic when annealed; slight ferromagnetism after heavy cold work or after sigma-phase formation

Do not skip the expansion number. At ~16 ×10⁻⁶ /K, 310S expands about a third more than carbon steel and 10–15 % more than 304, while its thermal conductivity is only about a third of carbon steel's. The combination — high expansion, poor conduction — produces thermal gradients and thermal stress, and it is the single most common reason furnace fixtures and radiant tubes crack: not loss of strength, but thermal fatigue from restrained expansion.

High-temperature performance: oxidation, scaling and creep

  • Oxidation / scaling: in clean, dry, oxidizing atmospheres the 25 % Cr scale is protective to about 1,150 °C in continuous service, and to about 1,035 °C where thermal cycling causes the scale to spall and re-form. Cycling is the enemy: every spall-and-reheat cycle consumes chromium from the metal, and a part that is fine in continuous duty can fail in a few hundred cycles.
  • Creep and rupture: below ~550 °C, 310S and 310H behave identically. Above that, carbon content governs — 310H is the grade for structural furnace parts, tube supports, hangers and radiant tubes where the design is limited by deformation over 10,000–100,000 h. Specify 310H when your design temperature exceeds roughly 600 °C and the part carries load.
  • Carburization: moderate. In carbon-bearing atmospheres (endothermic gas, CO, hydrocarbon cracking) 310S eventually carburizes and becomes brittle; 800H/HT or 601 resist better, and 693 is the answer for severe carburizing/oxidizing alternation.
  • Sulphidation and reducing atmospheres: poor. H2S, SO2-rich or low-oxygen atmospheres destroy the chromium oxide scale; use 600/601/693 or a nickel-chromium grade with higher Ni.
  • Molten salts and metals: not recommended in contact with molten aluminium, zinc or copper alloys; 310S is attacked and can contaminate the melt.
  • Cryogenic: fully austenitic and tough — 310S is one of the few high-Cr grades also used at cryogenic temperature, since it has no ductile-brittle transition.

Atmosphere rule of thumb: clean oxidizing air, continuous, no load → 310S to 1,100–1,150 °C. Load-bearing above 600 °C → 310H. Thermal cycling with scale spall, or sulphur in the gas → leave the 300 series and go to 601 or 693. Reducing or carburizing atmospheres are never 310S territory, whatever the temperature.

Sigma phase, sensitisation and the 600–900 °C trap

This is where most 310S failures originate, and it is entirely predictable. Between roughly 600 and 900 °C — fastest around 750–850 °C — the high chromium content that makes 310S heat-resistant also makes it willing to precipitate sigma phase, a hard, brittle intermetallic at the grain boundaries. The consequences are a sharp drop in room-temperature ductility and impact toughness, a slight rise in magnetism, and reduced corrosion resistance. A furnace part that ran happily at 1,050 °C for years can shatter on cooldown after a spell in the sigma window, or crack during a shutdown.

Temperature bandWhat happensDesign implication
425–860 °CSensitisation: chromium carbides precipitate at grain boundaries, chromium-depleting the adjacent metalAvoid slow cooling through this band after annealing or welding; use low-carbon 310S rather than high-carbon 310
600–900 °C (peak 750–850 °C)Sigma phase forms; toughness and ductility fall progressively over hundreds to thousands of hoursDo not design long-term service or slow-cool through this band; 310H is more susceptible than 310S but is used there only when creep governs and toughness is not needed
Above ~950 °CSigma dissolves; carbides go back into solutionSolution anneal at 1,040–1,150 °C and water-quench to restore ductility after service exposure

If a 310S part must operate in the 600–900 °C band, tell us at the enquiry stage. The usual answers are: accept a lower design stress and inspect for toughness, switch to a grade that does not form sigma as readily (309S is no better; 800H or 601 are), or design for replacement. Never rely on a room-temperature tensile test to prove a sigma-embrittled part is fit for purpose — impact testing is the only meaningful check.

Aqueous corrosion — what 310S is not for

  • Nitric acid: excellent. High chromium and no molybdenum make 310S one of the better stainless grades in hot nitric acid, and it is used for nitric-acid plant internals and nuclear reprocessing equipment.
  • General oxidizing media: good; the high Cr content gives a robust passive film and good resistance to general corrosion and to high-temperature oxidation products.
  • Chloride stress-corrosion cracking: good, thanks to 20 % nickel — considerably better than 304 or 316, though not in the immunity class of the 33 %+ Ni alloys.
  • Pitting and crevice corrosion: weak. With no molybdenum and no nitrogen, PREN (Cr + 3.3 Mo + 16 N) is only about 25 — barely better than 304. Seawater, brackish water and chloride brines will pit it; that is not what this grade is for.
  • Intergranular corrosion: moderate susceptibility. 310S at 0.08 % C is far safer than 310 at 0.25 % C, but a welded 310S assembly in a sensitising acid service should still be solution-annealed or tested to ASTM A262.
  • Reducing acids (HCl, dilute H2SO4): poor. Molybdenum-free austenitics have little resistance; use 316L, 904L or a Ni-Mo grade.

Typical applications by industry

IndustryTypical 310S / 310H componentsWhy this grade
Heat treatment & furnacesMuffles, retorts, annealing boxes, baskets, trays, fixtures, radiant tubes, fan shafts, roller railsScaling resistance to ~1,150 °C plus structural stability — no phase transformation on cycling
Boilers & powerSuperheater and reheater tube supports, hangers, spacers, burner nozzles, soot-blower partsCreep strength (310H) and oxidation resistance in flue gas
Cement, lime & ceramicsKiln internals, preheater cyclones, burner tips, kiln nose rings, saggar and kiln furnitureHot strength and resistance to alkali/oxide dust at 900–1,100 °C
Petrochemical & refiningFurnace tube supports, transfer-line hangers, coke-drum internals, catalyst-bed gridsHigh-temperature strength with weldability
Chemical processingNitric-acid equipment, high-temperature reactor internals, catalyst supports, thermocouple protection tubesNitric acid and oxidizing service plus heat
Waste incineration & environmentalGrate bars, ash-handling parts, flue ducting, thermal-oxidizer internalsOxidation resistance at temperature; not for the aggressive HCl/alkali zones
Automotive & aerospace ground equipmentExhaust manifolds for heavy-duty and stationary engines, heat shields, test-rig ductingThermal fatigue resistance in cyclic hot gas
Cryogenic & specialLNG and cryogenic vessel internals, superconducting magnet structureRetains toughness at low temperature — no DBTT

Standards and product forms

Product formASTM / ASME specification
Plate, sheet, stripASTM A240 / ASME SA240
Bar, rod, wireASTM A276 / A479
Seamless and welded pipeASTM A312 / ASME SA312
Seamless and welded tubeASTM A213 / A249 / A269
Welded fittingsASTM A403 WP310
CastingsASTM A351 CK20 / A297 HK
Welding consumablesER310 (AWS A5.9), E310 (A5.4); ERNiCr-3 for dissimilar joints
European designationW.Nr 1.4845, X8CrNi25-21
Asian designationsJIS SUS310S, GB/T 06Cr25Ni20, KS STS310S

Note the W.Nr trap: 1.4845 covers both 310S and 310H because the European standard no longer separates them by carbon band in the same way as ASTM. If your specification is written in EN terms, add the UNS number and the carbon range explicitly. 1.4841 is a different steel (314, with ~2 % Si) and is not interchangeable.

Fabrication, welding and heat treatment

  • Solution annealing: 1,040–1,150 °C, then water quench or rapid air cool. This dissolves carbides and sigma and restores ductility. Do not slow-cool through 600–900 °C.
  • Hot working: start at 1,150–1,200 °C and finish above 950 °C; re-anneal after hot working rather than cooling in air from the finishing temperature.
  • Cold forming: high work-hardening rate — comparable to 304 but with higher flow stress. Anneal between severe operations; formed parts for high-temperature service should be annealed before going into the furnace, otherwise the cold-worked structure recrystallizes in service and distorts.
  • Machining: gummy and work-hardening; carbide tooling, positive rake, generous depth of cut, no dwelling.
  • Welding: use ER310 (25/20) matching filler for 310-to-310 joints. The fully austenitic weld metal is prone to solidification cracking, so keep heat input low, use stringer beads, control the bead profile (slightly convex), and avoid high restraint. For dissimilar joints to carbon steel or to lower-alloy stainless, ER309 or a nickel filler (ERNiCr-3) is more tolerant.
  • Preheat and PWHT: no preheat, no post-weld heat treatment. A PWHT in the 600–900 °C range would do exactly the damage the grade is designed to avoid — it would precipitate sigma and sensitize the HAZ.
  • Backing and cleaning: purge with argon for tube and pipe roots; pickling and passivation after welding restores the oxide film and removes heat tint, which is a corrosion initiator in aqueous service.
  • Service-side caution: support long horizontal furnace parts at close intervals — creep sag, not fracture, is the usual end of life for 310S/310H fixtures. Design for 1 % creep strain over the expected campaign, not for ultimate strength.

Purchasing checklist

CheckWhat to look for
Grade identityUNS S31008 (310S) or S31009 (310H) stated on the PO and certificate — never just "310", which permits 0.25 % carbon
Carbon310S: ≤ 0.08 %; 310H: 0.04–0.10 %. This is the only way to distinguish the two — PMI cannot
Chromium / nickelCr 24.0–26.0 %, Ni 19.0–22.0 %; be suspicious of material sitting at the bottom of both ranges
ConditionSolution annealed, with the annealing temperature and cooling method stated
Grain sizeFor creep-critical 310H, agree a grain size (typically ASTM 4 or coarser) — fine grains creep faster
Intergranular testASTM A262 Practice E on request for welded assemblies in corrosive service
CertificatesEN 10204 3.1 plus PMI; UT for pressure-boundary plate; dimensional check to A480
SurfaceNo embedded iron, no grinding burn; pickled finish for furnace parts that will be cycled

Buying 310S / 310H from Hangbo

We supply 310S and 310H as plate, sheet, bar, seamless and welded pipe, tube, fittings and machined furnace furniture, cut to size and, where needed, formed and welded to drawing. Stock sizes normally ship in 7–15 days; mill-rolled plate and heat-specific 310H orders run 30–45 days. Tell us the design temperature, the atmosphere (oxidizing, carburizing, sulphur-bearing), whether the part carries load and whether it cycles — those four answers decide between 310S, 310H, 309S, 314 or a nickel-base grade, and we would rather steer you to the right one before you buy than replace a cracked retort afterwards.

Frequently asked questions

Should I order 310S or 310H?

Order 310S for sheet, ducting and non-load-bearing parts and for anything welded that will see aqueous or mildly corrosive service — the lower carbon resists sensitisation. Order 310H when the part carries load above roughly 600 °C and the design is limited by creep: tube supports, hangers, radiant tubes, kiln internals. Room-temperature properties are the same, so the decision is purely about temperature and load.

What is the maximum service temperature of 310S?

About 1,150 °C in clean, dry, oxidizing gas under continuous duty, and about 1,035 °C where thermal cycling causes scale to spall. In load-bearing applications the limit is set by creep, not oxidation, and falls to roughly 900–1,000 °C depending on stress. Reducing, carburizing or sulphur-bearing atmospheres cut the usable temperature much further — in those cases move to 601 or 693.

Can 310S be used in seawater?

No. Its PREN is only about 25 because it contains no molybdenum or nitrogen, so pitting and crevice corrosion start quickly in chloride water. For seawater use a 6 % Mo super-austenitic (254SMO, AL-6XN) or a duplex/super duplex grade.

Is 310S magnetic?

It is non-magnetic in the annealed condition. Slight magnetism after heavy cold working or bending is normal and harmless. Strong magnetism on a part that has been in high-temperature service is a warning sign of sigma phase or of a wrong grade — check the certificate and consider impact testing.

Does 310S need post-weld heat treatment?

No — and it usually should not get one. A stress relief in the 600–900 °C range would precipitate sigma phase and sensitise the heat-affected zone. The correct post-weld treatment, if any, is a full solution anneal at 1,040–1,150 °C with rapid cooling, which is impractical on large fabrications and therefore designed around.

310S or 309S or 314 — how do I choose?

309S (22 Cr / 13 Ni) is the cheaper step down, adequate to about 980 °C and often used for furnace supports that are not heavily loaded. 310S extends oxidation resistance to ~1,150 °C and is the default for 1,000–1,100 °C work. 314 adds about 2 % silicon for better scaling resistance and higher creep strength but is harder to weld and much less available.

Need 310S / 310H (UNS S31008 / S31009)?

Send us your drawing or specification for a quotation — we reply within one business day.

Request a quote