[email protected] WhatsApp +86 159 0085 2030 Qingpu, Shanghai Reply within 1 business day

Nimonic 90 (UNS N07090): composition, properties and applications

Nimonic 90 is what happens when you take the proven Nimonic 80A recipe and add 15–21 % cobalt: the gamma-prime phase becomes stable at higher temperature and coarsens more slowly, buying roughly 100 °C of extra creep capability. The result is a Ni-Cr-Co-Ti-Al alloy rated for creep-resisting duty to about 920 °C — the classic choice for turbine blades, discs and high-temperature springs where 80A margins run out. This guide covers the composition, aged values, physical data and the purchasing details that matter when quoting 90 in bar, forgings, rings and spring wire.

Stainless steel seamless tubes in warehouse

What Nimonic 90 is — in one paragraph

Nimonic 90 (UNS N07090, W.Nr 2.4969 / 2.4632) is an age-hardenable nickel-chromium-cobalt alloy: the Nimonic 80A base of ~20 % Cr and Ti+Al gamma-prime formers, plus 15–21 % cobalt dissolved in the matrix. Cobalt raises the gamma-prime solvus and slows its coarsening at temperature, so the alloy carries higher creep loads and keeps its strength roughly 100 °C hotter than 80A — useful creep-resisting service to about 920 °C. It reaches that strength only after the full heat treatment (solution ~1,080 °C + age ~700 °C), and it is available in the wrought forms that turbines and spring-makers need: bar, forgings, rolled rings and, distinctively for this grade, high-temperature spring wire.

Nominal chemical composition

ElementContent (wt %)Why it matters
Nickel (Ni)BalanceAustenitic matrix, high-temperature stability
Cobalt (Co)15–21The defining addition: raises the γ′ solvus, slows precipitate coarsening, adds solid-solution strength
Chromium (Cr)18–21Oxidation resistance in hot combustion gas
Titanium (Ti)2–3Primary gamma-prime former — sets the strengthening volume fraction
Aluminium (Al)0.7–1.3Second γ′ former (AMS/BS bands run slightly wider than DIN)
Carbon (C)0.13 maxControlled carbides for grain-boundary behaviour
Iron (Fe)1.5–3.0 max (spec-dependent)Residual — keep low for full creep performance
Silicon / Manganese1.0 max eachMelting-process control
Zirconium (Zr) / Boron (B)0.15 / 0.010–0.020 maxGrain-boundary strength against creep rupture

Chemistry bands differ slightly between DIN 17744 (NiCr20Co18Ti), AMS 5829 and the BS HR specifications — most visibly for Al and Fe. State the governing specification at enquiry; it determines the melt route and the guaranteed test results on the certificate.

Mechanical properties

Room-temperature values for bar and forgings, by heat-treatment condition:

ConditionYield strength (0.2 %)Tensile strengthElongation
Solution treated (DIN 17744 specified minimum)≥ 590 MPa≥ 820 MPa—
Solution treated + aged (typical mill values)≈ 800–810 MPa≈ 1,200–1,240 MPa≈ 20 %

Creep-rupture data published for 1,000 h gives roughly 200 MPa at 750 °C and about 80 MPa at 850 °C — the numbers that justify choosing 90 over 80A when the design sits above ~800 °C. In drawn wire the picture changes completely: cold-drawn 90 spring wire reaches 1,300–1,500 MPa tensile before ageing and higher after it, which is precisely why the grade dominates high-temperature spring applications. As always with age-hardened alloys, a solution-treated forging and an aged forging from the same heat give very different values — the condition must be stated explicitly on the order.

Physical properties

PropertyValue
Density8.18 g/cm³
Melting range≈ 1,310–1,365 °C (some mill datasheets quote 1,310–1,370 °C)
Thermal conductivity (20 °C)≈ 11–11.5 W/m·K
Specific heat≈ 410–460 J/kg·K (sources differ — confirm on the mill datasheet)
Thermal expansion (20–100 °C)≈ 12.7–12.8 ×10⁻⁶ /K
Modulus of elasticity (20 °C)≈ 206–220 GPa (sources differ)
Electrical resistivity≈ 1.18–1.25 µΩ·m
Magnetic behaviourEssentially non-magnetic in the solution-treated condition

Use these for quoting, weight calculation and thermal design allowances. They are typical published values, not guaranteed properties — guaranteed values are agreed at order stage and reported on the EN 10204 certificate issued with each heat.

High-temperature performance — the cobalt difference

  • Creep duty to ≈ 920 °C: cobalt keeps the γ′ dispersion fine at temperatures where 80A's precipitates have already coarsened, extending useful creep-resisting and stress-rupture service by roughly 100 °C.
  • 1,000 h rupture strength: ≈ 200 MPa at 750 °C, ≈ 80 MPa at 850 °C — a real margin over 80A in exactly the band where industrial-turbine bolting and blading live.
  • Spring performance at temperature: drawn wire holds its coil load where ordinary spring alloys sag — springs, retaining rings and lockwire stay elastic at temperatures that would anneal steel springs soft.
  • Above the limit: beyond ~920 °C oxidation and γ′ coarsening end the design life; cast superalloys or higher-alloyed wrought grades take over.

Selection rule of thumb: 718 tops out near 650 °C for creep, 80A carries you to ~815 °C, Nimonic 90 to ~920 °C. If your design is rupture-limited above ~800 °C and 80A margins are thin, 90 is the next rung on the same metallurgical ladder — same heat-treatment logic, same fabrication discipline, ~100 °C more headroom.

Typical applications

IndustryTypical 90 components
Gas & steam turbinesHP turbine blades, discs, rotor rings, blade roots, spacers, seal rings
Aerospace enginesCombustor casing rings, afterburner components, shafts, mounting flanges
Springs & fastenersHigh-temperature spring wire, retaining rings, lockwire, hot bolting that must hold preload at 700–900 °C
Oil, gas & offshoreWellhead and compressor hardware needing creep stability at elevated temperature
Valves & flow controlValve stems, seat rings and bonnets in hot gas and steam service
Exhaust & powerExhaust valves and turbocharger components carrying higher thermal loads than 80A duties

Standards and product forms we supply

  • Bars, forgings and rings: ASTM B637 / ASME SB637, UNS N07090
  • Aerospace: AMS 5829 (forgings), MSRR 7137 / 7017, AECMA prEN 2295 / 2296 / 2298 / 2299
  • European: W.Nr 2.4969 / 2.4632, DIN 17744 (NiCr20Co18Ti), DIN 17752, BS HR 2
  • China: GB GH4090 (GH90)
  • Forms: round bar, forging stock, rolled rings, discs, and drawn wire for springs — cut or machined to drawing
  • Certification: EN 10204 3.1 standard; 3.2 with TÜV/SGS/BV/LR witness arranged on request

Heat treatment, welding and purchasing notes

Heat treatment. The standard cycle for bar and forgings is solution treatment at 1,080 °C (typically 8 h), air cool, then precipitation ageing at 700 °C for 16 h, air cool. Sheet routes and some aerospace specifications use different solution and stabilisation stages — state the governing specification if a non-standard cycle is required. Springs are coiled from hard-drawn wire and then aged to set the final strength.

Welding. As with all γ′-hardened Nimonic grades, weld in the solution-treated condition and age afterwards where the specification allows; welding an aged part risks strain-age cracking in the HAZ. Matching wire is crack-sensitive, so fabricators commonly use ERNiCr-3 / ENiCr-3 filler for joining and repair, accepting that the weld metal will not match aged parent strength. Design load paths so the weld is not the creep-critical section.

Purchasing. Specify: delivery condition (solution treated vs solution treated + aged), governing standard (B637 / AMS 5829 / DIN 17744 / BS HR 2), melt route — EAF+VOD+ESR as standard, VIM+VAR or VIM+ESR for aerospace classes — plus grain-size and ultrasonic acceptance for rotating parts. The alloy work-hardens fast and machines best in the solution-treated condition with rigid setups and carbide or ceramic tooling; age after rough machining to hold final dimensions.

Frequently asked questions

What is the difference between Nimonic 90 and Nimonic 80A?

One word: cobalt. 90 carries 15–21 % Co against 80A's essentially cobalt-free composition, which raises the gamma-prime solvus and slows its coarsening. That buys roughly 100 °C of extra creep capability (~920 °C vs ~815 °C) and somewhat higher aged strength — at a higher alloy cost.

Is Nimonic 90 magnetic?

No — it is essentially non-magnetic in the solution-treated condition and remains effectively non-magnetic when aged. A strong magnet response suggests the wrong material.

Can Nimonic 90 replace Alloy 718?

Above ~650 °C, yes — 718 loses creep strength quickly there (and suffers δ-phase embrittlement), while 90 keeps working to ~920 °C. Below 650 °C, 718 is the better buy: cheaper, far more weldable, and stronger at room temperature. Match the grade to the operating temperature, not the brochure.

Why is Nimonic 90 so popular for springs?

Drawn 90 wire reaches very high tensile strengths (1,300–1,500 MPa and above after ageing) while staying elastic at 700–900 °C, where steel and ordinary nickel springs lose their set. It is the standard high-temperature spring, retaining-ring and lockwire alloy in turbines and engines.

What should I specify on the purchase order?

The condition (solution treated vs solution treated + aged), the governing standard, the melt route (ESR minimum for forged rings and discs; VIM for aerospace classes), and any grain-size, UT or 3.2-witness testing. Unstated conditions are the single biggest source of disputes with age-hardened alloys.

Need Nimonic 90 (UNS N07090)?

Send us your drawing or specification for a quotation — we reply within one business day.

Request a quote