[email protected] WhatsApp +86 159 0085 2030 Qingpu, Shanghai Reply within 1 business day

Invar 36 (UNS K93600): composition, properties and applications

Invar 36 is the alloy that made 'dimensional stability' a materials spec rather than a hope. With 36 % nickel balance iron, its thermal expansion between roughly 20 and 100 °C is about 1.3–1.5 ×10⁻⁶/K — a tenth of carbon steel — and it holds that behaviour from cryogenic temperature up to about 260 °C. That single property makes it the default choice for aerospace composite curing tooling, LNG containment and precision instruments. This guide covers the data behind the alloy, and the thermal-expansion fine print that separates a good Invar purchase from an expensive lesson.

What Invar 36 is — in one paragraph

Invar 36 (UNS K93600/K93603, W.Nr 1.3912; also sold as Alloy 36 and Nilo 36) is a nickel-iron controlled-expansion alloy containing 35.0–37.0 % nickel with iron as the balance. Discovered by Charles Édouard Guillaume in 1897 — a result that earned the 1920 Nobel Prize in Physics — the alloy's near-zero expansion comes from a magnetically driven volume compensation below its Curie point: thermal expansion is almost exactly cancelled by magnetostrictive contraction, so the net coefficient collapses to roughly one-tenth that of carbon steel. The alloy keeps good strength and toughness at cryogenic temperature, which is why LNG membrane systems and liquid-nitrogen hardware sit alongside aerospace composite tooling in its application list. Note that the low-expansion behaviour is ferromagnetic in origin: Invar 36 is magnetic at room temperature, and the effect disappears at the Curie point (≈ 230 °C).

Nominal chemical composition

Composition limits per ASTM F1684 and the Rolled Alloys data sheet; the nickel content is the controlling element and iron is the balance:

ElementContent (wt %)Why it matters
Nickel (Ni)35.0–37.0The expansion-controlling element — the Invar effect peaks near 36 % Ni at ambient temperature
Iron (Fe)BalanceMatrix of the ferromagnetic compensation mechanism
Carbon (C)0.10 maxKept low for stability; carbides would disturb the expansion behaviour
Manganese (Mn)0.60 maxDeoxidation
Silicon (Si)0.35 maxDeoxidation and processing control
Copper (Cu)0.50 maxResidual control
Chromium / Molybdenum (Cr, Mo)0.50 max eachResidual limits — both raise CTE if allowed to accumulate
Phosphorus / Sulfur (P, S)0.025 max eachPurity limits for consistent magnetic behaviour

The UNS K93603 variant (Astroloy-free high-purity melt, e.g. for vacuum/electron-device work) carries tighter residual limits — if your application is laser mounts, shadow masks or hermetic devices, ask for K93603 rather than standard K93600.

Mechanical properties

Typical room-temperature values for the annealed condition per the Rolled Alloys and open-die forging data sheets, with the spread quoted by independent suppliers in brackets:

ConditionTensile strengthYield strength (0.2 %)Elongation
Annealed (typical)490 MPa [430–550]240 MPa [240–350]42 % [25–42]
1/4 hard (cold-worked strip/bar)620–793 MPa——
1/2 hard (cold-worked strip/bar)724–862 MPa——
Hard (cold-worked)827 MPa min——

Strength falls off gently with temperature — published mill data show the annealed alloy retaining roughly 60 ksi tensile at 150 °C and about 30 ksi at 600 °C — but nobody buys Invar 36 for hot strength. Hardness in the annealed state is typically 130–180 HB, and the elastic modulus is around 141 GPa (sources quote 138–148), noticeably softer than steel. These are typical values, not guaranteed minima; your heat's test results appear on the EN 10204 certificate.

Physical properties

PropertyValue
Density≈ 8.1 g/cm³ (0.293 lb/in³; some suppliers quote 8.05)
Melting point≈ 1,427–1,430 °C
Thermal expansion (20–100 °C, annealed)≈ 1.3–1.5 ×10⁻⁶ /K — about one-tenth of carbon steel
Thermal conductivity≈ 10–11 W/m·K (sources vary; not a design-critical value for this alloy)
Electrical resistivity≈ 0.84 µΩ·m
Elastic modulus≈ 141 GPa
Curie point≈ 230 °C (sources quote 220–280 °C depending on composition)
Magnetic behaviourFerromagnetic at room temperature and throughout the low-expansion range

Thermal expansion behaviour — the fine print that matters

The headline number (≈ 1.5 ×10⁻⁶/K) applies near room temperature only. The coefficient rises steadily with temperature and then jumps once the ferromagnetic compensation switches off at the Curie point. Published data (Rolled Alloys, per 70 °F reference; ZYTC per 30 °C) agree well:

Temperature rangeCTE (×10⁻⁶ /K)
20–100 °C≈ 1.3–1.5
30–200 °C≈ 1.7
30–250 °C≈ 2.5
30–300 °C≈ 4.9
30–400 °C≈ 7.8

Selection rule of thumb: the low-expansion service window runs from cryogenic temperature to about 260 °C (500 °F). Above ≈ 230 °C (Curie point) the Invar effect collapses and the alloy expands like ordinary steel. For service hotter than that, you need a different controlled-expansion alloy, not more Invar. And because the mechanism is magnetic, CTE also depends on the anneal cycle and cold work — for precision tooling, specify the annealed condition and, where the drawing warrants it, a measured CTE test report.

Typical applications

IndustryTypical Invar 36 components
Aerospace / compositesCuring tooling, molds and fixtures for carbon-fibre lay-up — tool and part expand together, so net-shape accuracy survives the autoclave cycle
LNG / cryogenicsMembrane tank components, cryogenic piping and supports for liquefied gas service below −162 °C
Optics / laserOptical benches, laser component mounts, cavity resonators, telescope structures
Metrology / instrumentsLength standards, pendulum rods, precision measuring devices, scientific (seismic/accelerator) equipment supports
ElectronicsShadow masks, hermetic device housings (K93603), thermostat element pairings

Standards and product forms we supply

  • Sheet, strip, plate, bar, wire, forgings: ASTM F1684 (the commonly cited specification for the wrought alloy), ASTM B753 (strip/foil grades), SEW 385, AFNOR NF A54-301 (chemistry)
  • UNS designations: K93600 (standard), K93603 (high purity for electronic/vacuum service)
  • Supply forms: round bar, sheet, plate, strip, wire and open-die forgings; forged rings and blocks are quoted to drawing with EN 10204 3.1 certificates
  • Weld consumables: filler metal CF36 bare wire for GTAW and GMAW

Machining, welding and procurement notes

Machining: Invar 36 cuts like a soft austenitic stainless steel — which is to say gummily. Use sharp, positive-rake tools, generous coolant and avoid rubbing; heavy cold work at the surface can locally perturb expansion behaviour, so finish cuts should be light. Stress-relief annealing after rough machining is standard practice on precision tooling before final machining.

Heat treatment: the annealing cycle (typically 830–900 °C, slow cool) sets the grain structure and stabilises the CTE. If a drawing specifies dimensional stability, the anneal condition and thermal cycle are part of the specification — not an afterthought.

Welding: readily weldable with CF36 filler (GTAW/GMAW). Match the filler to the application: in composite tooling, weld areas should be ground flush and the assembly re-annealed where stability matters.

Procurement discipline: Invar 36 is bought for one property, so the PO should carry more than a UNS number. Specify the product form and standard (F1684/B753), the annealed condition, and — for tooling and metrology parts — a maximum CTE at 20–100 °C with a test report. Magnetic response is normal and is not a rejection criterion.

Frequently asked questions

Is Invar 36 magnetic?

Yes — it is ferromagnetic at room temperature and throughout the low-expansion range, with a Curie point around 230 °C. Magnetism is intrinsic to the Invar effect; a magnetic response does not indicate a wrong or defective alloy.

What is the maximum service temperature for low expansion?

About 260 °C (500 °F). The CTE stays low from cryogenic temperature up to that window, then rises sharply as the ferromagnetic compensation switches off near the Curie point (≈ 230 °C) — above roughly 300 °C the alloy behaves like ordinary steel expansion-wise.

Invar 36 vs Alloy 42 — which one do I need?

Invar 36 wins where near-zero expansion near ambient temperature matters (tooling, optical benches, LNG). Alloy 42 (Ni 42 %, UNS K94100) has a higher CTE (≈ 4–5 ×10⁻⁶/K) deliberately matched to silicon and ceramics, and is the standard choice for glass-to-metal seals and semiconductor lead frames. Pick by what you need to match, not by which number looks smaller.

Can Invar 36 be welded, and does welding ruin the expansion behaviour?

It welds readily with CF36 filler wire by GTAW or GMAW. The weld metal and HAZ see a different thermal cycle than the parent metal, so for precision tooling the accepted practice is to machine flush after welding and, where the stability budget demands it, re-anneal the assembly before final machining.

Need Invar 36 / Alloy 36 (UNS K93600)?

Send us your drawing or specification for a quotation — we reply within one business day.

Request a quote